Next Article in Journal
Fatigue Behavior of Linear Friction Welded Ti-6Al-4V and Ti-6Al-2Sn-4Zr-2Mo-0.1Si Dissimilar Welds
Next Article in Special Issue
Structure, Magnetocaloric Effect and Critical Behavior of the Fe60Co12Gd4Mo3B21 Amorphous Ribbons
Previous Article in Journal
A Novel Dry Treatment for Municipal Solid Waste Incineration Bottom Ash for the Reduction of Salts and Potential Toxic Elements
Previous Article in Special Issue
Determination of Phase Transition and Critical Behavior of the As-Cast GdGeSi-(X) Type Alloys (Where X = Ni, Nd and Pr)
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Tuning of the Structure and Magnetocaloric Effect of Mn1−xZrxCoGe Alloys (Where x = 0.03, 0.05, 0.07, and 0.1)

Department of Physics, Częstochowa University of Technology, Armii Krajowej 19, 42-200 Częstochowa, Poland
*
Author to whom correspondence should be addressed.
Submission received: 7 May 2021 / Revised: 31 May 2021 / Accepted: 3 June 2021 / Published: 7 June 2021

Abstract

:
The aim of the present work is to study the influence of a partial substitution of Mn by Zr in MnCoGe alloys. The X-ray diffraction (XRD) studies revealed a coexistence of the orthorhombic TiNiSi-type and hexagonal Ni2In- type phases. The Rietveld analysis showed that the changes in lattice constants and content of recognized phases depended on the Zr addition. The occurrence of structural transformation was detected. This transformation was confirmed by analysis of the temperature dependence of exponent n given in the relation ΔSM = C·(BMAX)n. A decrease of the Curie temperature with an increase of the Zr content in the alloy composition was detected. The magnetic entropy changes were 6.93, 13.42, 3.96, and 2.94 J/(kg K) for Mn0.97Zr0.03CoGe, Mn0.95Zr0.05CoGe, Mn0.93Zr0.07CoGe, and Mn0.9Zr0.1CoGe, respectively. A significant rise in the magnetic entropy change for samples doped by Zr (x = 0.05) was caused by structural transformation.

1. Introduction

The magnetocaloric effect (MCE) is the change of temperature of magnetic material under the variations of an external magnetic field. This effect is manifested as the cooling or heating of magnetic materials under the influence of an alternating magnetic field [1]. The MCE is observed in all magnetic materials. It is the result of the coupling of the magnetic field with the magnetic subnetwork, which leads to a change in the magnetic part of the entropy of the solid [2]. This phenomenon is described as the adiabatic temperature change (∆Tad) or magnetic entropy change (∆SM).
The most popular magnetocaloric materials include pure Gd and its alloys [3], La(Fe, Si)13 alloys [4,5], and manganites [6]. The magnetocaloric effect is observed in a group of alloys called Heusler alloys. This is a group of chemical compounds and alloys. Recently, research has focused on full Heusler [7] and half Heusler [8] alloys, such as: (MnNiGe)1−x-(FeCoGe)x [9], Co1−xCuxMnSb [10], NiFeSb [11], CoV1−xMnSb, NiTi1−xMnxSb [12], Co(Mn, Nb)Sb [13], (Zr0.5Hf0.5)Co(Sb0.85Sn0.15) [14], MnFeP1−xAxx [15], and MnCoGe [16].
The general formula for describing full Heusler alloys is: X2YZ, where X and Y are atoms from the subgroup (transition metal), and Z is atoms from the main group (metalloids) [17]. The characteristic feature of the full Heusler is: 2: 1: 1 stoichiometry, the structure of the Cu2MnAl type, as well as the Fm 3 ¯ m space group (No. 225, L21). The structure of L21 consists of four interpenetrating cubic subnets with a face-centered (fcc) [18]. The atoms are in the following positions: A—4a (0, 0, 0), B—4b (0.5, 0.5, 0.5), and C—8c (0.25, 0.25, 0.25). Metals are most often included among these alloys [19]. The structure of a full Heusler is shown in Figure 1.
The general formula for half-Heusler alloys is: XYZ. Characteristic features of this type of alloy include 1:1:1 stoichiometry, structure of the MgAgAs type, as well as the F 4 ¯ 3m space group (No. 216, C1b). The structure of C1b is obtained by removing one location of the X atom from the L21 structure [18]. The half-Heusler alloy atoms are in the following positions: A—4a (0, 0, 0), B—4b (0.5, 0.5, 0.5), and C—4c (0.25, 0.25, 0.25). These alloys include most often semiconductors [20]. The half-Heusler structure is shown in Figure 2.
The influence of partial substitution of Mn by Zr was previously studied in [21,22]. Qian and coworkers showed the possibility of the induction of martensitic transition for the specific composition of the (Mn,Zr)CoGe alloy. However, they did not present complete analysis of the order of phase transition or i.e., values of the refrigeration capacity. In order to broaden the knowledge concerning on this group of materials, we decided to study them. The aim of the present study was to investigate the effect of the substitution of Mn by Zr in the MnCoGe alloy on the structure, magnetic properties, and phase transition.

2. Sample Preparation and Experimental Details

Samples with the nominal composition of Mn1−xZrxCoGe, where x = 0.03, 0.05, 0.07, and 0.1, were prepared using the arc melting method of high purity elements in an Ar protective gas atmosphere. The samples were remelted several times in order to ensure their homogeneity. The X-ray diffraction (XRD) studies were performed using a Bruker D8 Advance diffractometer (Bruker, Karlruhe, Germany) with CuKα radiation and a LynxEye semiconductor detector (Bruker, Karlruhe, Germany). The collected X-ray pattern was analyzed with the Bruker EVA software (4.3). The Rietveld analysis was conducted using the PowderCell 2.4 package [23]. Magnetic measurements were carried out using the Quantum Design Physical Properties Measuring System (PPMS) model 6000, equipped to work with a wide range of magnetic fields and temperatures.

3. Results and Discussion

The room temperature XRD patterns were measured for all investigated samples and are presented in Figure 3. For the Mn0.97Zr0.03CoGe alloy sample, the dominant hexagonal Ni2In- type phase was detected with small amount of the orthorhombic NiTiSi-type phase. A similar phase composition was observed for samples of the Mn0.95Zr0.05CoGe alloy. An intensive growth of the orthorhombic NiTiSi-type phase, at the expense of the Ni2In- type phase, was observed for samples doped with Zr for x = 0.07 and x = 0.1. Qian and coworkers in [22] showed that the partial substitution of Mn by Zr caused lowering of the temperature of structural transition and induced the formation of the hexagonal Ni2In-type phase.
However, current studies confirmed the results described in [21]. A slight increase of lattice constants is visible with an increase of the Zr content in the alloy composition. Such an effect was expected due to the ionic radius of Zr (rZr = 1.60 Å) being higher than Mn (rZr = 1.18 Å), and this causes expansion of the orthorhombic and hexagonal phases. Considering that the orthorhombic structure could be considered as a distorted hexagonal cell [24], an addition of Zr promotes the formation of the NiTiSi-type phase. Deep analysis of the XRD patterns did not detect any additional phase related to an occurrence of impurities. The Rietveld analysis carried out using experimental XRD patterns revealed some slight changes in the lattice constants of recognized phases. The results of the Rietveld refinement were collected in Table 1.
Johnson in [25] showed relations between the unit cells of these two structures as:
a o r t h = c h e x b o r t h = a h e x c o r t h = 3 a h e x
Figure 4 presents the dependence between lattice parameters versus the Zr content of the hexagonal and orthorhombic structure for the studied samples. It is clearly seen that the orthorhombic phase changed by 11% along the a axis during the orthorhombic-hexagonal structural transition. At the same time, this lattice enlarged by 6.5% and 0.02% along the b and c axes, respectively. An occurrence of structural transformation significantly affected the value of the magnetic entropy change. The obtained values correspond well with the results delivered in [22,26]. As it was shown by Gschneidner and coworkers in [27], such a structural transformation could increase ΔSM by even 90%.
To measure the Curie point, the temperature dependences of magnetization were collected in a magnetic field of 0.01 T for all studied samples (Figure 5). The Curie temperature was revealed by calculations of the first derivative of the M = f(T) curves. The estimated values of the TC were 290, 285, 283, and 278 K for Mn0.97Zr0.03CoGe, Mn0.95Zr0.05CoGe, Mn0.93Zr0.07CoGe, and Mn0.9Zr0.1CoGe, respectively. The gradual decrease of the TC was observed, which is expected in accordance with previous studies [15,21]. Such behavior could also be caused by lowering of the magnetic moment of Mn by Zr during mixing as was shown in [28].
The magnetocaloric effect was studied indirectly by calculations of the magnetic entropy change ΔSM. In order to calculate the ΔSM values, the magnetic isotherms were measured for a wide range of temperatures. The calculations of magnetic entropy change were realized using the Maxwell relation [29]:
Δ S M ( T , Δ H ) = μ 0 0 H ( M ( T , H ) T ) H d H
where μ0 is the magnetic permeability, H is the magnetic field strength, M is the magnetization, and T is the temperature.
Equation (2) was implemented in Mathematica software using the following algorithm:
Δ S M ( T i + T i + 1 2 ) 1 T i + 1 T i [ 0 B max M ( T i + 1 , B ) d B 0 B max M ( T i , B ) d B ]
where B is the magnetic field induction according to the relation B = μ0H.
The temperature evolution of the magnetic entropy change is presented in Figure 6. The highest values of the ΔSM calculated for the change of external magnetic field ~5 T, were 6.93, 13.42, 3.96, and 2.94 J/(kg K) for Mn0.97Zr0.03CoGe, Mn0.95Zr0.05CoGe, Mn0.93Zr0.07CoGe, and Mn0.9Zr0.1CoGe, respectively (Figure 7). In comparison to the results reported for the MnCoGe-based alloy presented in [21], the Zr addition caused a slight decrease of the ΔSM. However, a further increase to x = 0.05 induced a significant rise of the magnetic entropy change. Moreover, the asymmetric shape of the ΔSM vs. T curve for the Mn0.95Zr0.05CoGe alloy sample suggests that such a relevant increase was caused by a magnetostructural first order phase transition.
Further increases of the Zr content in the alloy composition caused a decrease of the ΔSM. The values of magnetic entropy change are comparable with those reported in [26] However, these values are almost two times lower than results presented by Qian et al. [22]. Moreover, for samples with the highest Zr content (x = 0.07 and 0.1), a significant broadening of the ΔSM peak was noticed.
In order to conduct more deep characterization of the magnetocaloric properties, the refrigeration capacity was calculated using the following relation [30]:
RC ( δ T , H MAX ) = T cold T hot Δ S M ( T , H MAX ) d T
where RC is the refrigerant capacity, δT = Thot − Tcold is the temperature range of the thermodynamic cycle (δT corresponds to the full width at half maximum of magnetic entropy change peak), and HMAX is the maximum value of the external magnetic field.
The highest value of the RC was reached for the sample with the Zr content x = 0.05. This was caused by the relatively high value of the magnetic entropy change. In the case of other studied alloys, the RCs were similar. The values of magnetic entropy change ΔSM and refrigeration capacity RC are collected in Table 2.
As it was mentioned above, the significant rise of magnetic entropy change could be related to the first order phase transition. An interesting and relatively fast technique to investigate the order of phase transition was proposed by Law et al., which could be called the Law–Franco method [31]. This technique is based on the phenomenological field dependence of magnetic entropy change proposed by Franco in [32] and described by the following relation:
Δ S M = C ( B MAX ) n
where C is a constant depending on temperature and n is the exponent related to the magnetic state of sample. The n exponent can be easily calculated by modification of Equation (5) in the form proposed in [33]:
ln Δ S M = ln C + n ln B MAX
The n exponent is strongly dependent on the magnetic state [34]. If a material obeys the Curie law, the exponent n = 1 in the ferromagnetic state (below TC), and n = 2 in the paramagnetic state (above TC). The exponent n value at the Curie point is described by the relation:
n = 1 + 1 δ ( 1 1 β )
where β and δ are critical exponents.
The temperature dependences of exponent n are presented in Figure 8 for all studied samples. In the case of samples with Zr contents x = 0.03, 0.07, and 0.1, the n vs. T curves are typical for the second order phase transition. Moreover, the values revealed in the vicinity of the TC amount of 0.74, 0.76, and 0.73, for Mn0.97Zr0.03CoGe, Mn0.93Zr0.07CoGe, and Mn0.9Zr0.1CoGe, respectively. These values are similar, which suggests that values of critical exponents are close to others. However, the n vs. T curve constructed for Mn0.95Zr0.05CoGe is typical for samples, which manifest a first order phase transition and structural transformation [31,35]. An occurrence of a structural peak in the vicinity of 275 K corresponds very well to the peak in the differential scanning calorimetry (DSC) curve presented in [22].

4. Conclusions

In this paper, we investigated the effect of the partial substitution of Mn by Zr in the MnCoGe alloys on the structure and magnetic properties. The coexistence of the orthorhombic TiNiSi-type phase and hexagonal Ni2In- type phases was found for all investigated samples. Moreover, the XRD studies supported by the Rietveld analysis allowed us to detect the structural transformation. We found a gradual decrease in the Curie temperature with the increase of the Zr content in the alloy composition. For the sample with Zr content x = 0.05, a significant increase of the magnetic entropy change was achieved, induced by a magnetostructural phase transition. In the case of other samples, the gradual decrease of the ΔSM was calculated. The analysis of the temperature dependence of exponent n ( Δ S M = C ( B MAX ) n ) proved an occurrence of a magnetostructural transition in the Mn0.95Zr0.05CoGe alloy sample.

Author Contributions

Conceptualization, K.K. and P.G.; methodology, K.K.; validation, P.G.; formal analysis, K.K. and P.G.; investigation, K.K. and P.G.; writing—original draft preparation, K.K. and P.G.; writing—review and editing, K.K. and P.G.; supervision, P.G.; funding acquisition, P.G. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Tishin, A.M.; Spichkin, Y.I. The Magnetocaloric Effect and Its Applications; Institute of Physics Series in Condensed Matter Physics: London, UK, 2003. [Google Scholar]
  2. Pecharsky, V.K.; Gschneidner, K.A., Jr. Magnetocaloric effect and magnetic refrigation. J. Magn. Magn. Mater. 1999, 200, 44–56. [Google Scholar] [CrossRef]
  3. Yue, M.; Zhang, J.; Zeng, H.; Chen, H.; Liu, X.B. Magnetocaloric effect in Gd5Si2Ge2/Gd composite materials. J. Appl. Phys. 2006, 99, 08Q104. [Google Scholar] [CrossRef]
  4. Fujita, A.; Akamatsu, Y.; Fukamichi, K. Itinerant electron metamagnetic transition in La(FexSi1−x)13 intermetallic compounds. J. Appl. Phys. 1999, 85, 4756–47568. [Google Scholar] [CrossRef]
  5. Gebara, P.; Kovac, J. The influence of partial substitution of La by Dy on structure and thermomagnetic properties of the LaFe11.0Co0.7Si1.3 alloy. J. Magn. Magn. Mater. 2018, 454, 298–303. [Google Scholar] [CrossRef]
  6. Zhong, W.; Cheng, W.; Ding, W.P.; Zhang, N.; Du, Y.W.; Yan, Q.J. Magnetocaloric properties of Na-Substituted perovskite-Type magnese oxides. Solid State Commun. 1998, 106, 55–58. [Google Scholar] [CrossRef]
  7. He, A.; Svitlyk, V.; Mozharivskyj, Y. Synthetic Approach for (Mn,Fe)2(Si,P) Magnetocaloric Materials: Purity, Structural, Magnetic, and Magnetocaloric Properties. Inorg. Chem. 2017, 56, 2827–2833. [Google Scholar] [CrossRef]
  8. Koller, M.; Chraska, T.; Cinert, J.; Heczko, O.; Kopecek, J.; Landa, M.; Musalek, R.; Rames, M.; Siner, H.; Strasky, J.; et al. Mehcanical and magnetic properties of semi-Heusler/light-metal composites consolidated by spark plasma sintering. Mater. Des. 2017, 126, 351–357. [Google Scholar] [CrossRef]
  9. Kuang, Y.; Yang, B.; Hao, X.; Xu, H.; Li, Z.; Yan, H.; Zhang, Y.; Esling, C.; Zhao, X.; Zuo, L. Gigant low field magnetocaloric effect near room temperature in isostructurally alloyed MnNiGe-FeCoGe systems. J. Magn. Magn. Mater. 2020, 506, 166782. [Google Scholar] [CrossRef]
  10. Duong, N.P.; Hung, L.T.; Hien, T.D.; Thuy, N.P.; Trung, N.T.; Bruck, E. Magnetic properties of half-metallic semi Heusler Co1−xCu xMnSb compounds. J. Magn. Magn. Mater. 2007, 311, 605–608. [Google Scholar] [CrossRef]
  11. Zhang, M.; Liu, Z.; Hu, H.; Cui, Y.; Liu, G.; Chen, J.; Wu, G.; Sui, Y.; Qian, Z.; Li, Z.; et al. A new semi-Heusler ferromagnet NiFeSb: Electronic structure, magnetism and transport properties. Solid State Commun. 2003, 128, 107–111. [Google Scholar] [CrossRef]
  12. Pierre, J.; Kaczmarska, K.; Tobola, J.; Skolozdra, R.V.; Melnyk, G.A. Location of Mn 3d states in semi-Heusler compounds. Physica B 1999, 261, 841–842. [Google Scholar] [CrossRef]
  13. Wu, X.Y.; Zhang, J.; Yuan, H.K.; Kuang, A.L.; Chen, H. Effect of Nb doping on electronic and magnetic properties of half-metallic CoMnSb semi-Heusler compound from first-principles calculations. Phys. Status Solid B 2010, 247, 945–949. [Google Scholar] [CrossRef]
  14. Heinz, S.; Balke, B.; Jakob, G. Hole localization in thermoelectric half-Heusler (Zr0.5Hf0.5)Co(Sb1−xSnx) thin films. Thin Solid Film 2019, 692, 137581. [Google Scholar] [CrossRef]
  15. Bruck, E.; Ilyn, M.; Tishin, A.M.; Tegus, O. Magnetocaloric effects in MnFeP1−xAsx-based compounds. J. Magn. Magn. Mater. 2005, 291, 8–13. [Google Scholar] [CrossRef]
  16. Trung, N.T.; Zhang, L.; Caron, L.; Buschow, K.H.J.; Bruck, E. Gigant magnetocaloric effect by tailoring the phase transitions. Appl. Phys. Lett. 2010, 96, 172504. [Google Scholar] [CrossRef]
  17. Morán-López, J.; Rodriguez-Alba, R.; Aguilera-Granja, F. Modeling the magnetic properties of Heusler alloys. J. Magn. Magn. Mater. 1994, 131, 417–426. [Google Scholar] [CrossRef]
  18. Beloufa, A.; Bakhti, B.; Bouguenna, D.; Chellali, M.R. Computational investigation of CrFeZ [Z = Si, Sn and Ge] half-Heusler compounds ferromagnets. Phys. B Condens. Matter 2019, 563, 50–55. [Google Scholar] [CrossRef]
  19. Graf, T.; Casper, F.; Winterlik, J.; Balke, B.; Fecher, G.H.; Felser, C. Crystal Structure of New Heusler Compounds. Z. Anorg. Allg. Chem. 2009, 635, 976–981. [Google Scholar] [CrossRef] [Green Version]
  20. Hohl, H.; Ramirez, A.P.; Goldmann, C.; Ernst, G.; Wölfing, B.; Bucher, E. New Compounds with MgAgAs-type structure: NbIrSn and NbIrSb. J. Phys. Condens. Matter. 1998, 10, 7843. [Google Scholar] [CrossRef]
  21. Gębara, P.; Śniadecki, Z. Structure, magnetocaloric properties and thermodynamic modeling of enthalpies of formation of (Mn,X)-Co-Ge (X=Zr, Pd) alloys. J. Alloys Compd. 2019, 796, 153–159. [Google Scholar] [CrossRef]
  22. Qian, F.; Zhu, Q.; Miao, X.; Fan, J.; Zhong, G.; Yang, H. Tailoring the magneto-structural coupling in Mn1−xZrxCoGe alloys. J. Mater. Sci. 2021, 56, 1472–1480. [Google Scholar] [CrossRef]
  23. Kraus, W.; Nolze, G. PowderCell 2.0 for Windows. Powder Diffr. 1998, 13, 256. [Google Scholar]
  24. Bażela, W.; Szytuła, A.; Todorović, J.; Tomkowicz, Z.; Zieba, A. Crystal and magnetic structure of NiMnGe. Phys. Status Solid A 1976, 38, 721–729. [Google Scholar] [CrossRef]
  25. Johnson, V. Diffusionless orthorhombic to hexagonal transitions in ternary silicides and germanides. Inorg. Chem. 1975, 14, 1117–1120. [Google Scholar] [CrossRef]
  26. Li, G.J.; Liu, E.K.; Zhang, H.G.; Zhang, Y.J.; Chen, J.L.; Wang, W.H.; Zhang, H.W.; Wu, G.H.; Yu, S.Y. Phase diagram, ferromagnetic martenstic transformation and magnetoresposive properties of Fe-doped MnCoGe alloys. J. Magn. Magn. Mater. 2013, 332, 146–150. [Google Scholar] [CrossRef] [Green Version]
  27. Gschneidner, K.A.J.; Mudryk, Y.; Pecharsky, V.K. On the nature of the magnetocaloric effect of the first-order magnetostructural transition. Scr. Mater. 2012, 67, 572–577. [Google Scholar] [CrossRef]
  28. Hauser, J.J.; Waszczak, J.V. Spin-glass transition in MnO. Phys. Rev. B 1984, 30, 5167–5171. [Google Scholar] [CrossRef]
  29. Pecharsky, V.K.; Gschneider, K.A. Magnetocaloric effect from indirect measurements: Magnetization and heat capacity. Jr. J. Appl. Phys. 1999, 86, 565–575. [Google Scholar] [CrossRef]
  30. Wood, M.E.; Potter, W.H. General analysis of magnetic refrigeration and its optimization using a new concept: Maximization of refrigerant capacity. Cryogenics 1985, 25, 667–683. [Google Scholar] [CrossRef]
  31. Law, J.Y.; Franco, V.; Moreno-Ramírez, L.M.; Conde, A.; Karpenkov, D.Y.; Radulov, I.; Skokov, K.P.; Gutfleisch, O. A quantitative criterion for determining the order of Magnetic phase transitions using the magnetocaloric effect. Nat. Commun. 2018, 9, 2680. [Google Scholar] [CrossRef]
  32. Franco, V.; Conde, A.; Provenzano, V.; Shull, R. Scaling analysis of the magnetocaloric effect in Gd5Si2Ge1.9X0.1 (X=Al, Cu, Ga, Mn,Fe,Co). J. Magn. Magn. Mater. 2010, 322, 218–223. [Google Scholar] [CrossRef]
  33. Skokov, K.P.; Müller, K.-H.; Moore, J.D.; Liu, J.; Karpenkov, Y.A.; Krautz, M.; Gutfleisch, O. Influence of thermal hysteresis and field cycling on themagnetocaloric effect in LaFe11.6Si1.4. J. Alloys Compd. 2013, 552, 310–317. [Google Scholar] [CrossRef]
  34. Morrison, K.; Sandeman, K.G.; Cohen, L.F.; Sasso, C.P.; Basso, V.; Barcza, A.; Katter, M.; Moore, J.D.; Skokov, K.P.; Gutfleisch, O. Evaluation of the reliability of the measurement of key magnetocaloric properties: A round robin study of La(Fe,Si, Mn)Hdconducted by the SSEEC consortium of European laboratories. Int. J. Refrig. 2012, 35, 1528–1536. [Google Scholar] [CrossRef] [Green Version]
  35. Gębara, P.; Hasiak, M. Determination of Phase Transition and Critical Behavior of the As-Cast GdGeSi-(X) Type Alloys (Where X = Ni, Nd and Pr). Materials 2021, 14, 185. [Google Scholar] [CrossRef]
Figure 1. Full Heusler alloy structure model [19].
Figure 1. Full Heusler alloy structure model [19].
Materials 14 03129 g001
Figure 2. Half-Heusler alloy structure model [20].
Figure 2. Half-Heusler alloy structure model [20].
Materials 14 03129 g002
Figure 3. The XRD patterns collected for all studied samples.
Figure 3. The XRD patterns collected for all studied samples.
Materials 14 03129 g003
Figure 4. The Zr content dependence of the lattice constant of the analyzed unit cells. Errors were not matched as they were smaller than the symbol size. (a) Zr content of lattice parameters (aort and chex); (b) Zr content of lattice parameters (ahex, bort and cort/(3)1/2).
Figure 4. The Zr content dependence of the lattice constant of the analyzed unit cells. Errors were not matched as they were smaller than the symbol size. (a) Zr content of lattice parameters (aort and chex); (b) Zr content of lattice parameters (ahex, bort and cort/(3)1/2).
Materials 14 03129 g004
Figure 5. The temperature dependences of magnetization collected under the external magnetic field of 0.01 T for all studied samples. Values were normalized to their maximum value.
Figure 5. The temperature dependences of magnetization collected under the external magnetic field of 0.01 T for all studied samples. Values were normalized to their maximum value.
Materials 14 03129 g005
Figure 6. The temperature dependences of the magnetic entropy changes calculated for Mn0.97Zr0.03CoGe (a), Mn0.95Zr0.05CoGe (b), Mn0.93Zr0.07CoGe (c), and Mn0.9Zr0.1CoGe (d) alloys.
Figure 6. The temperature dependences of the magnetic entropy changes calculated for Mn0.97Zr0.03CoGe (a), Mn0.95Zr0.05CoGe (b), Mn0.93Zr0.07CoGe (c), and Mn0.9Zr0.1CoGe (d) alloys.
Materials 14 03129 g006
Figure 7. The temperature dependences of the magnetic entropy changes calculated for Mn0.97Zr0.03CoGe (a), Mn0.95Zr0.05CoGe (b), Mn0.93Zr0.07CoGe (c), and Mn0.9Zr0.1CoGe (d) alloys under the change of external magnetic field ~5 T.
Figure 7. The temperature dependences of the magnetic entropy changes calculated for Mn0.97Zr0.03CoGe (a), Mn0.95Zr0.05CoGe (b), Mn0.93Zr0.07CoGe (c), and Mn0.9Zr0.1CoGe (d) alloys under the change of external magnetic field ~5 T.
Materials 14 03129 g007
Figure 8. The temperature dependences of the exponent n calculated for all investigated samples.
Figure 8. The temperature dependences of the exponent n calculated for all investigated samples.
Materials 14 03129 g008
Table 1. The results of the Rietveld analysis for all investigated samples.
Table 1. The results of the Rietveld analysis for all investigated samples.
AlloyCrystalline PhaseLattice Parameter [Å] ± 0.001Volume Fraction [%]
Mn0.97Zr0.03CoGehex Ni2In- typea = 4.07293
c = 5.282
ort NiTiSi- typea = 5.9397
b = 3.825
c = 7.052
Mn0.95Zr0.05CoGehex Ni2In- typea = 4.07392
c = 5.283
ort NiTiSi- typea = 5.9408
b = 3.825
c = 7.053
Mn0.93Zr0.0.07CoGehex Ni2In- typea = 4.07982
c = 5.284
ort NiTiSi- typea = 5.94018
b = 3.827
c = 7.054
Mn0.9Zr0.1CoGehex Ni2In- type a = 4.08172
c = 5.285
ort NiTiSi- typea = 5.94128
b = 3.827
c = 7.055
Table 2. The magnetic entropy change ΔSM and refrigerant capacity RC for the Mn0.97Zr0.03CoGe, Mn0.95Zr0.05CoGe, Mn0.93Zr0.07CoGe, and Mn0.9Zr0.1CoGe alloys.
Table 2. The magnetic entropy change ΔSM and refrigerant capacity RC for the Mn0.97Zr0.03CoGe, Mn0.95Zr0.05CoGe, Mn0.93Zr0.07CoGe, and Mn0.9Zr0.1CoGe alloys.
AlloyΔ(μ0H) [T]ΔSM [J (kg K)−1]RC [J kg−1]
Mn0.97Zr0.03CoGe11.3829
23.1867
34.4192
45.51139
56.93195
Mn0.95Zr0.05CoGe12.6437
26.3499
38.71174
412.02296
513.42425
Mn0.93Zr0.07CoGe11.1341
21.7371
32.46114
43.33165
53.96246
Mn0.9Zr0.1CoGe10.6633
21.3578
31.97121
42.42177
52.94219
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Kutynia, K.; Gębara, P. Tuning of the Structure and Magnetocaloric Effect of Mn1−xZrxCoGe Alloys (Where x = 0.03, 0.05, 0.07, and 0.1). Materials 2021, 14, 3129. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14113129

AMA Style

Kutynia K, Gębara P. Tuning of the Structure and Magnetocaloric Effect of Mn1−xZrxCoGe Alloys (Where x = 0.03, 0.05, 0.07, and 0.1). Materials. 2021; 14(11):3129. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14113129

Chicago/Turabian Style

Kutynia, Karolina, and Piotr Gębara. 2021. "Tuning of the Structure and Magnetocaloric Effect of Mn1−xZrxCoGe Alloys (Where x = 0.03, 0.05, 0.07, and 0.1)" Materials 14, no. 11: 3129. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14113129

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop