Next Article in Journal
Impact of Bias Temperature Instabilities on the Performance of Logic Inverter Circuits Using Different SiC Transistor Technologies
Previous Article in Journal
Highly Conductive Ceramics with Multiple Types of Mobile Charge Carriers
Previous Article in Special Issue
Sapphire-Derived Fiber Bragg Gratings for High Temperature Sensing
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Growth and Characterization of Ce-Doped Luag Single Crystal Fibers from Transparent Ceramics by Laser-Heated Pedestal Method

1
Key Laboratory of Transparent Optical Functional Inorganic Materials, Shanghai Institute of Ceramics, Chinese Academy of Sciences, Shanghai 201899, China
2
Center of Materials Science and Optoelectronics Engineering, University of Chinese Academy of Sciences, Beijing 100049, China
*
Author to whom correspondence should be addressed.
Submission received: 14 July 2021 / Revised: 9 September 2021 / Accepted: 16 September 2021 / Published: 21 September 2021
(This article belongs to the Special Issue Crystalline Fibers and Their Applications)

Abstract

:
Scintillation single crystal fibers (SCFs) have great potential applications in the new generation of high-energy ray and particle detectors due to their morphological advantages. In this work; Ce:LuAG SCFs with a diameter of 1 mm were grown along the direction of [111] by laser-heated pedestal growth (LHPG) method using a transparent ceramic as the source rod; and a doping concentration was 0.1 at%, 0.3 at%, 1 at%, respectively. The effects of growth rate and annealing in air on the scintillation and optical properties of SCF are discussed in detail. The results of analyzing the absorption spectra; radioluminescence (RL) spectra; pulse-height spectra and fluorescence lifetime of SCFs show that the SCF maintains excellent scintillation performance while having a fiber structure. Therefore; Ce:LuAG SCF is a potential candidate material for detector.

1. Introduction

At present, inorganic scintillation materials have been widely studied because of their irreplaceable role in the fields of high energy physics, medical imaging and nuclear energy technology, etc. [1,2,3,4]. In addition to the traditional inorganic scintillation crystals BGO and NaI [5], which have been widely used, YAG [6], LuAG [7], YAP [8], and Lu2SiO5, Lu2-xYxSiO5 (LSO, LYSO) [9,10] and Y2SiO5 (YSO) [11] have also been rapidly developed under the promotion of application requirements. In addition, some new perspective materials such as Bi2O3-Na2O-TiO2-ZnO-TeO2 [12] and Bi Coatings [13] also show good performance in radiation shielding and detection, but their application in detectors is not very mature. Among them, Ce:LuAG has relatively high density, high effective atomic number (ρ = 6.7 g/cm3, Zeff = 60), short decay time (~50 ns), high theoretical light yield (25,000 photons MeV−1) [14,15,16], and good mechanical and chemical stability. Moreover, the wide emission of 5d-4f radiative transition of Ce3+ at 530 nm matches the spectral sensitivity of photodetectors used in high energy physics very well [17], so Ce:LuAG is considered to be one of the representatives of a new generation of scintillator crystals. Table 1 [5] summarizes the properties of commonly used scintillator materials. It can be seen from Table 1 that the light yield of Ce3+ doped LuAG crystal is comparable to that of LYSO crystal. In addition, the short radiation length (1.41 cm) and the proper interaction length (23.3 cm) of LuAG crystal can provide a large enough stopping power for the hadron energizer. LuAG crystals are excellent Cherenkov radiators with short absorption edge (177 nm), large transmission ratio and high refractive index (1.84) [18]. Caltech conducted neutron and proton irradiation experiments on Ce:LuAG, and found that Ce:LuAG has the best antiradiation performance among the materials known at present, and the ab-sorption coefficient of neutron and proton irradiation is only half of that of LYSO [19]. These outstanding advantages make LuAG crystals an ideal candidate for future high energy physics, especially for high irradiation backgrounds.
The current methods for growing LuAG single crystals mainly include Czochralski (CZ) [20,21], Bridgman (BD) [22,23] and micro-pulling-down (μ-PD) [24,25]. Among them, the CZ method and BD can be used for growing large crystals, but the utilization rate is low and the cost is higher. Although the μ-PD method can grow fibrous LuAG crystals, reducing the production cost of the material, the crucible is needed during the growth process, and the high melting point of LuAG crystals will inevitably bring pollution into the growth process. Another main method for growing inorganic SCFs is the LHPG method. Compared with the above three crystal preparation methods, the biggest advantage of the LHPG method is that it does not need to use a crucible during the growth process. The laser beam directly irradiates the top of the raw material rod to form a melting zone, and then under the traction of the seed crystal, it uses its own surface tension to maintain stability. Its advantages are as follows: (1) it can reduce the impurity pollution caused by the crucible during the growth process; (2) it can grow SCF with a smaller diameter without crucible limitation; (3) its melting zone is small and has a high temperature gradient, so the crystal growth rate is faster. At the same time, preparing the scintillation crystal into a fiber shape can facilitate the construction of a scintillator array detector, which makes up for the limitation of the sensitivity of the electromagnetic probe due to the low effective Z value of the atomic components in the application of plastic/organic scintillator fiber. For example, A. Benaglia [26] developed the Ce:LuAG scintillation array detector and tested the detection performance of high-energy rays with an energy range of 50~150 GeV. M. Nikl [27] also worked on the preparation and research of scintillation SCF.
In this work, we successfully prepared Ce:LuAG SCFs by using the LHPG method, and systematically characterized its scintillation performance. The results show that the Ce:LuAG scintillation crystal still has good scintillation performance after fiberation.

2. Materials and Methods

2.1. Growth of Single Crystal Fibers

The equipment information about LHPG method has been introduced in literature [28]. The source rod used in the growth process of the LHPG method can be either crystal or ceramic. In this work, we used a transparent ceramic as the source rod. The preparation process of transparent ceramics is explained in the literature [29]. The transparent ceramic was cut into a square rod with a section of 1.5 × 1.5 mm2, and one end of the rod was sharpened with LuAG in <111> direction as the seed crystal. In the high purity nitrogen atmosphere, the ceramic source rod is placed in an appropriate position, so that the CO2 laser can form a stable melting zone on its top, as shown in Figure 1a. The seed crystal is slowly placed in the melting zone and the laser is adjusted to the appropriate power. The appropriate fiber diameter can be obtained by controlling the ratio of the seed lifting speed Vf to the source rod feeding speed VS. This ratio is generally ½–1/3 [30]. To maintain the dimension and quality of the SCFs, according to experience, we chose a source rod feeding speed of 8 mm/h and 16 mm/h, respectively to grow 1 mm diameter SCFs. According to the law of the conservation of mass, we can easily calculate a crystal growth rate of 22.5 mm/h and 45 mm/h, respectively (slightly smaller than the calculated value to compensate for the density difference between the transparent ceramics and the crystal).
Using transparent ceramic as the source rod, we grew Ce:LuAG SCFs with doping concentrations of 0.1 at%, 0.3 at% and 1 at%, respectively. The length of the fibers could exceed 200 mm. After being cut into Φ1 × 3 mm3, the fibers were put into muffle furnace to rise to 1400 °C at 50 °C/h, and annealed in air for 30 h. The growing SCFs and the transparent ceramic used are shown in Figure 2.

2.2. Characterization

The absorption spectra within the range of 200~800 nm of Ce:LuAG SCFs were collected on a Lambda750 UV/VIS/NIR spectrometer using a resolution setting of 1 nm at room temperature and the size of samples was Ø = 1 × 2.5 mm3. The radioluminescence (RL) measurements were performed on an X-ray Excited Luminescence (XEL) Spectrometer built by Shanghai Institute of Ceramics, Chinese Academy of Science. An X-ray tube (F30III-2, V = 50 kV and I = 500 mA) equipped with a tungsten target was applied as the excitation source. The Hamamatsu R928 photomultiplier tube was used as a detector. The pulse-height (energy) spectra were recorded by an ORTEC digiBASE multichannel spectrometer. The sample with the size of Ø = 1 × 4 mm3 was excited by 662 KeV gamma ray from a 137Cs source. The SCF was optically coupled to the light entrance window of the PMT R6233 with an optical grease. The high voltage was supplied by ORTEC 556 high voltage power supply, and signals were read out from the anode of PMT. Then, the signals passed ORTEC 570 shaping amplifier with 10 μs shaping time, and were converted to digital signals by a Pocket MCA 8000 A multi-channel analyzer (MCA) provided by Amptek Co. Nanosecond flashing light was used as the excitation source. The fluorescence lifetimes were recorded by the spectrofluorometer under 447 nm excitation (FLS980PL Edinburgh).

3. Results and Discussion

3.1. Spectral Properties

Figure 3 and Figure 4 reveal the effects of growth rate, Ce ion concentration and annealing on the absorption spectra and X-ray excitation emission spectra of Ce:LuAG SCFs. It can be seen from Figure 3a that Ce:LuAG SCFs still retain the basic properties of crystals. The absorption peaks at 350 nm and 450 nm correspond to 4f–5d transition of Ce3+ ions.
As can be seen from Figure 3b, the absorption coefficient of SCF with a slower growth rate is greater than that of SCF with a faster growth rate at the same concentration. In combination with Figure 4b, it can also be found that SCF with a faster growth rate has a higher luminous intensity. From Figure 4b, the luminescence associated with the antisite of Lu-Al can be detected in the UV region [31] and it can be seen that the luminous intensity is higher when the growth rate is faster, so the rapid growth can inhibit the generation of antilocation defects to a certain extent. In turn, it affects the absorption intensity and emission intensity. However, it can be predicted that if the growth rate is too fast, other types of defects will easily occur that will affect SCF luminescence. Combined with Figure 3c and Figure 4c, it can be seen that with the increase in Ce ion concentration, both its absorption and excitation spectra gradually increase. Combined with Figure 3d and Figure 4d, it can be seen that annealing has little effect on the absorption intensity, but the emission intensity of 1 at% Ce:LuAG decreases, and that of 0.3 at% Ce:LuAG increases, while that of 0.1 at% Ce:LuAG almost remains unchanged. The possible reason is that we use transparent ceramic as the source rod, which contains Mg2+ and other fluxing agents, so some Ce4+ ions will be generated. After annealing in the air, the Ce3+ ions will be reduced and then its luminescence will be weakened, but defects will also be reduced and the luminescence intensity will be increased. As for 1 at% Ce:LuAG, there are more defects due to the excessive content of Ce ions. After annealing, only some of the defects are eliminated, but the content of Ce4+ will greatly increase, resulting in a decrease in the luminescence intensity. The content of the Ce4+ ion in 0.3 at% Ce:LuAG increases somewhat after annealing, but the defects are greatly reduced after annealing and the luminescence intensity increases due to its low concentration. The content of Ce4+ ions in 0.1 at% Ce:LuAG has increased, which weakens the luminescence, but also eliminates some defects and enhances the luminescence. The luminescence intensity is almost constant after they have cancelled each other out.

3.2. Scintillation Properties of Ce:LuAG SCF

Figure 5a shows the pulse height spectra of all samples. As can be seen from Figure 5b, the number of channels in the pulse height spectra of SCF with fast growth rate at the same concentration is slightly increased. It means that light yield increases, corresponding to the spectral properties mentioned above. It can be seen from Figure 5c that doping with different concentrations has little effect on the track number of pulse height spectra. It can be clearly seen in Figure 5d that the trace number of pulse height spectra increases after annealing at different concentrations. This is because annealing can increase the content of Ce4+ ions and reduce defects such as vacancy and residual stress generated by growth in nitrogen atmosphere. All of these are beneficial to increase its light yield. The energy resolution (ER) was calculated using the full width at half maximum (FWHM) and the MCA channel number value of the peak obtained from the Gauss fit of the full energy peak area. The calculated FWHM, peak and energy resolution are shown in Table 2.
Figure 6 shows the fluorescence decay curve corresponding to Ce3+ 5d–4F transition in Ce:LuAG SCFs under different conditions. A single exponential equation was used to fit the data, and the fluorescence lifetime was also listed in the Figure 6 and Table 2. It can be seen that it has the same decay curve as transparent ceramics [31]. Is the characteristic decay time of 5d–4F transition of Ce3+. Compared with the results of the fluorescence spectrum, it can be seen that when the growth rate is faster, the luminescence intensity is slightly increased, and the corresponding decay time is slightly increased or unchanged, which may be because the rapid growth rate cannot only inhibit the inverse defects, but also produce other types of defects that affect the fluorescence attenuation. At the same concentration and the same growth rate, the emission decay time of 1 at% Ce:LuAG is slightly increased after annealing, while the emission decay time of 0.3 at% Ce:LuAG and 0.1 at% Ce:LuAG is slightly decreased, which may be due to the increase in Ce4+ after annealing in air, so the decay time is faster [31]. However, due to the high doping concentration in 1 at%, there are many defects which cannot be completely eliminated by annealing. At the same time, Ce4+ itself does not emit light. After annealing, Ce3+ ions are reduced, but Ce4+ is excessive, so its decay time is slightly increased.
According to the comprehensive properties and spectral properties in Table 2, under low concentration doping, faster growth rate (16 mm/h) and annealing can improve the scintillation performance of optical fibers. At the same time, the performance of Ce:LuAG grown by different growth methods was compared in Table 3 [3,31,32]. It can be seen from the table that the SCFs grown by LHPG method still retains the basic properties of single crystal. Moreover, Since there is no crucible restriction during the growth process, this method can also grow SCF with smaller diameter (≤200 μm) and longer length. Because of its large temperature gradient, it also has a faster growth rate than other methods.

4. Conclusions

In this paper, Ce:LuAG SCFs with a diameter of 1 mm and different Ce ion doping concentrations were successfully grown by the LHPG method using transparent ceramics as the source rod. The effects of different growth rates, concentrations and annealing on SCFs scintillation and optical properties were discussed in detail by analyzing the results of the X-ray excitation spectrum, fluorescence spectrum, lifetime and multichannel energy spectrum. The results show that, due to the characteristics of LHPG method, low concentration doping (0.3 at%, 0.1 at%), fast growth rate (45 mm/h) and the annealing process can improve the scintillation performance of SCFs. The scintillation properties of the grown SCFs are similar to those of single crystal and transparent ceramics. Therefore, the SCF retains the basic properties of bulk single crystal while having a fiber structure. In further work, we will grow SCFs with smaller diameters on the basis of this work and try to build scintillation array detectors with high spatial resolution by the SCF.

Author Contributions

Conceptualization: L.S. and A.W.; Investigation, X.W. and Z.L.; Writing—original draft, Y.D.; Writing—review & editing, Z.Z. and H.K. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the International Partnership Program of Chinese Academy of Sciences (121631KYSB20180045). This work was also supported by National Natural Science Foundation of China (51872309, U1832106, 61925508, 62005302), Science and Technology Commission of Shanghai Municipality (20511107400, ZJ2020-ZD-005) and Science Foundation for Youth Scholar of State Key Laboratory of High Performance Ceramics and Superfine Microstructures (SKL201904).

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Acknowledgments

Special thanks to Dongzhou Ding of Shanghai Institute of Ceramics, Chinese Academy of Sciences for the support in measuring the optical fiber scintillation performance.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Moszyński, M.; Ludziejewski, T.; Wolski, D.; Klamra, W.; Norlin, L. Properties of the YAG:Ce scintillator. Nucl. Instrum. Methods Phys. Res. Sect. A Accel. Spectrometers Detect. Assoc. Equip. 1994, 345, 461–467. [Google Scholar] [CrossRef]
  2. Van Eijk, C.W.E. Inorganic-scintillator development. Nucl. Instrum. Methods Phys. Res. Sect. A Accel. Spectrometers Detect. Assoc. Equip. 2001, 460, 1–14. [Google Scholar] [CrossRef]
  3. Djebli, A.; Boudjada, F.; Pauwels, K.; Kononets, V.; Patton, G.; Benaglia, A.; Lucchini, M.; Moretti, F.; Sidletskiy, O.; Dujardin, C.; et al. Growth and characterization of Ce-doped YAG and LuAG fibers. Opt. Mater. 2017, 65, 65–68. [Google Scholar] [CrossRef]
  4. Witkiewicz-Lukaszek, S.; Mrozik, A.; Gorbenko, V.; Zorenko, T.; Bilski, P.; Fedorov, A.; Zorenko, Y. LPE Growth of composite thermoluminescent detectors based on the Lu3−xGdxAl5O12:Ce single crystalline films and YAG:Ce Crystals. Crystals 2020, 10, 189. [Google Scholar] [CrossRef] [Green Version]
  5. Hu, C.; Zhang, L.Y.; Zhu, R.Y.; Demarteau, M.; Wagner, R.; Xia, L.; Xie, J.Q.; Li, X.; Wang, Z.H.; Shih, Y.H.; et al. Ultrafast inorganic scintillator-based front imager for Gigahertz Hard X-ray imaging. Nucl. Instrum. Methods Phys. Res. A 2019, 940, 223–229. [Google Scholar] [CrossRef]
  6. Kotaki, A.; Yoshino, M.; Yokota, Y.; Hanada, T.; Yamaji, A.; Toyoda, S.; Sato, H.; Ohashi, Y.; Kurosawa, S.; Kamada, K. Yoshikawa, A.Crystal growth and scintillation properties of tube shape-controlled Ce-doped Y3Al5O12 single crystals grown by micro-pulling-down method. Appl. Phys. Express 2020, 13, 125503. [Google Scholar] [CrossRef]
  7. Jiuping, Z.; Hongbin, L.; Qiang, S.; Guobin, Z.; Pieter, D.; Danang, B.M. Effects of Annealing Treatments on Luminescence and Scintillation Properties of Ce:Lu3Al5O12Crystal Grown by Czochralski Method. J. Rare Earths 2007, 25, 568–572. [Google Scholar] [CrossRef]
  8. Alshourbagy, M.; Bigotta, S.; Herbert, D.; Del Guerra, A.; Toncelli, A.; Tonelli, M. Optical and scintillation properties of Ce3+ doped YAlO3 crystal fibers grown by mu-pulling down technique. J. Cryst. Growth 2007, 303, 500–505. [Google Scholar] [CrossRef]
  9. Farhi, H.; Lebbou, K.; Belkahla, S.; Grosvalet, L.; Hautefeuille, B.; Caramanian, A.; Dujardin, C.; Tillement, O.; Pedrini, C. Fiber single crystal growth by LHPG technique and optical characterization of Ce3+-doped Lu2SiO5. Opt. Mater. 2008, 30, 1461–1467. [Google Scholar] [CrossRef]
  10. Hautefeuille, B.; Lebbou, K.; Dujardin, C.; Fourmigue, J.M.; Grosvalet, L.; Tillement, O.; Pedrini, C. Shaped crystal growth of Ce3+-doped Lu2(1-x)Y2xSiO5 oxyortho silicate for scintillator applications by pulling-down technique. J. Cryst. Growth 2006, 289, 172–177. [Google Scholar] [CrossRef]
  11. Koschan, M.; Yang, K.; Zhuravleva, M.; Melcher, C. A comparison of the effect of Ca2+ codoping in cerium doped GSO with that of LSO and YSO. J. Cryst. Growth 2012, 352, 133–136. [Google Scholar] [CrossRef]
  12. Sayyed, M.I.; Askin, A.; Zaid, M.H.M.; Olukotun, S.F.; Khandaker, M.U.; Tishkevich, D.I.; Bradley, D.A. Radiation shielding and mechanical properties of Bi2O3–Na2O–TiO2–ZnO–TeO2 glass system. Radiat. Phys. Chem. 2021, 186, 109556. [Google Scholar] [CrossRef]
  13. Tishkevich, D.I.; Grabchikov, S.S.; Lastovskii, S.B.; Trukhanov, S.V.; Zubar, T.I.; Vasin, D.; Trukhanov, A.V.; Kozlovskiy, A.; Zdorovets, M.M. Effect of the Synthesis Conditions and Microstructure for Highly Effective Electron Shields Production Based on Bi Coatings. ACS Appl. Energy Mater. 2018, 1, 1695–1702. [Google Scholar] [CrossRef]
  14. Derdzyan, M.V.; Ovanesyan, K.L.; Petrosyan, A.G.; Belsky, A.; Dujardin, C.; Pedrini, C.; Auffray, E.; Lecoq, P.; Lucchini, M.; Pauwels, K. Radiation hardness of LuAG:Ce and LuAG: Pr scintillator crystals. J. Cryst. Growth 2012, 361, 212–216. [Google Scholar] [CrossRef]
  15. Dujardin, C.; Mancini, C.; Amans, D.; Ledoux, G.; Abler, D.; Auffray, E.; Lecoq, P.; Perrodin, D.; Petrosyan, A.; Ovanesyan, K.L. LuAG:Ce fibers for high energy calorimetry. J. Appl. Phys. 2010, 108, 013510. [Google Scholar] [CrossRef]
  16. Petrosyan, A.G.; Ovanesyan, K.L.; Sargsyan, R.V.; Shirinyan, G.O.; Abler, D.; Auffray, E.; Lecoq, P.; Dujardin, C.; Pedrini, C. Bridgman growth and site occupation in LuAG:Ce scintillator crystals. J. Cryst. Growth 2010, 312, 3136–3142. [Google Scholar] [CrossRef]
  17. Di, J.Q.; Xu, X.D.; Xia, C.T.; Li, D.Z.; Zhou, D.H.; Wu, F.; Xu, J. Crystal growth and optical properties of LuYAG:Ce single crystal. J. Cryst. Growth 2012, 351, 165–168. [Google Scholar] [CrossRef]
  18. Auffray, D.; Abler, S.; Brunner, S.; Frisch, B.; Knapitsch, A.; Lecoq, P.; Mavromanolakis, G.; Poppe, O.; Petrosyan, A. LuAG Material for Dual Readout Calorimetry at Future High Energy Physics Accelerators. In Proceedings of the 2009 IEEE Nuclear Science Symposium Conference Record (NSS/MIC), Orlando, FL, USA, 24 October–1 November 2009; pp. 2245–2249. [Google Scholar]
  19. Hu, C.; Li, J.; Yang, F.; Jiang, B.; Zhang, L.; Zhu, R.-Y. LuAG ceramic scintillators for future HEP experiments. Nucl. Instrum. Methods Phys. Res. Sect. A Accel. Spectrometers Detect. Assoc. Equip. 2020, 954, 161723. [Google Scholar] [CrossRef]
  20. Kamada, K.; Yanagida, T.; Pejchal, J.; Nikl, M.; Endo, T.; Tsutsumi, K.; Usuki, Y.; Fujimoto, Y.; Fukabori, A.; Yoshikawa, A. Scintillation properties of Ce doped Gd2Lu(Ga,Al)5O12 single crystal grown by the micro-pulling-down method. J. Cryst. Growth 2012, 352, 35–38. [Google Scholar] [CrossRef]
  21. Sugiyama, M.; Fujimoto, Y.; Yanagida, T.; Yamaji, A.; Yokota, Y.; Yoshikawa, A. Growth and scintillation properties of Nd-doped Lu3Al5O12 single crystals by Czochralski and micro-pulling-down methods. J. Cryst. Growth 2013, 362, 178–181. [Google Scholar] [CrossRef]
  22. Tian, T.; Feng, H.; Zhang, Y.; Zhou, D.; Shen, H.; Wang, H.; Xu, J. Crystal Growth and Luminescence Properties of Dy3+ and Ge4+ Co-Doped Bi4Si3O12 Single Crystals for High Power Warm White LED. Crystals 2017, 7, 249. [Google Scholar] [CrossRef] [Green Version]
  23. Petrosyan, A.; Popova, V.; Gusarov, V.; Shirinyan, G.; Pedrini, C.; Lecoq, P. The Lu2O3–Al2O3 system: Relationships for equilibrium-phase and supercooled states. J. Cryst. Growth 2006, 293, 74–77. [Google Scholar] [CrossRef]
  24. Chani, V.; Lebbou, K.; Hautefeuille, B.; Tillement, O.; Fourmigue, J.-M. Evaporation induced diameter control in fiber crystal growth by micro-pulling-down technique: Bi4Ge3O12. Cryst. Res. Technol. 2006, 41, 972–978. [Google Scholar] [CrossRef]
  25. Wang, A.; Zhang, J.; Jia, Z.; Ye, S.; Ma, X.; Wu, B.; Wang, S.; Wang, F.; Wang, T.; Zhang, B. Optimized growth and laser application of yb:Luag single-crystal fibers by micro-pulling-down technique. Crystals 2021, 11, 78. [Google Scholar] [CrossRef]
  26. Benaglia, A.; Lucchini, M.T.; Pauwels, K.; Tully, C.; Medvedeva, T.; Heering, A.; Dujardin, C.; Kononets, V.; Lebbou, K.; Aubry, N.; et al. Test beam results of a high granularity LuAG fibre calorimeter prototype. J. Instrum. 2016, 11, P05004. [Google Scholar] [CrossRef] [Green Version]
  27. Nikl, M.; Yoshikawa, A. Recent R&D Trends in Inorganic Single-Crystal Scintillator Materials for Radiation Detection. Adv. Opt. Mater. 2015, 3, 463–481. [Google Scholar] [CrossRef]
  28. Dai, Y.; Zhang, Z.; Wang, Y.; Su, L.; Li, J.; Lo, C.; Wu, A. Growth of Tm:Lu3Al5O12 single crystal fiber from transparent ceramics by laser-heated pedestal method and its spectral properties. Opt. Mater. 2020, 111, 110674. [Google Scholar] [CrossRef]
  29. Liu, S.; Feng, X.; Hu, C.; Kou, H.; Li, J.; Mares, J.A.; Babin, V.; Nikl, M.; D’Ambrosio, C.; Pan, Y. Effect of Li+ ions co-doping on luminescence, scintillation properties and defects characteristics of LuAG:Ce ceramics. Opt. Mater. 2017, 64, 245–249. [Google Scholar] [CrossRef] [Green Version]
  30. Wang, T.; Zhang, J.; Zhang, N.; Wang, S.; Wu, B.; Jia, Z.; Tao, X. The characteristics of high-quality Yb:YAG single crystal fibers grown by a LHPG method and the effects of their discoloration. RSC Adv. 2019, 9, 22567–22575. [Google Scholar] [CrossRef] [Green Version]
  31. Liu, S.P.; Mares, J.A.; Feng, X.Q.; Vedda, A.; Fasoli, M.; Shi, Y.; Kou, H.M.; Beitlerova, A.; Wu, L.X.; D’Ambrosio, C.; et al. Towards Bright and Fast Lu3Al5O12:Ce,Mg Optical Ceramics Scintillators. Adv. Opt. Mater. 2016, 4, 731–739. [Google Scholar] [CrossRef]
  32. Yanagida, T.; Fujimoto, Y.; Yokota, Y.; Kamada, K.; Yanagida, S.; Yoshikawa, A.; Yagi, H.; Yanagitani, T. Comparative study of transparent ceramic and single crystal Ce doped LuAG scintillators. Radiat. Meas. 2011, 46, 1503–1505. [Google Scholar] [CrossRef]
Figure 1. (a) Hemispherical melting zone. (b) Trapezoidal melting zone.
Figure 1. (a) Hemispherical melting zone. (b) Trapezoidal melting zone.
Crystals 11 01149 g001
Figure 2. As-grown Ce:LuAG SCFs.
Figure 2. As-grown Ce:LuAG SCFs.
Crystals 11 01149 g002
Figure 3. (a) Absorption spectra of all Ce:LuAG SCFs; (b) Absorption spectra at different growth rates; (c) Absorption spectra at different concentrations; (d) Effect of annealing on absorption spectra.
Figure 3. (a) Absorption spectra of all Ce:LuAG SCFs; (b) Absorption spectra at different growth rates; (c) Absorption spectra at different concentrations; (d) Effect of annealing on absorption spectra.
Crystals 11 01149 g003
Figure 4. (a) Radioluminescence spectra of all Ce:LuAG SCFs; (b) Radioluminescence spectra at different growth rates; (c) Radioluminescence spectra at different concentrations; (d) Effect of annealing on radioluminescence spectra.
Figure 4. (a) Radioluminescence spectra of all Ce:LuAG SCFs; (b) Radioluminescence spectra at different growth rates; (c) Radioluminescence spectra at different concentrations; (d) Effect of annealing on radioluminescence spectra.
Crystals 11 01149 g004
Figure 5. (a) Pulse height spectra of all Ce:LuAG SCFs; (b) Pulse height of spectra at different growth rates; (c) Pulse height spectra at different concentrations; (d) Effect of annealing on R Pulse height spectra.
Figure 5. (a) Pulse height spectra of all Ce:LuAG SCFs; (b) Pulse height of spectra at different growth rates; (c) Pulse height spectra at different concentrations; (d) Effect of annealing on R Pulse height spectra.
Crystals 11 01149 g005
Figure 6. The fluorescence lifetimes of all Ce:LuAG SCFs.
Figure 6. The fluorescence lifetimes of all Ce:LuAG SCFs.
Crystals 11 01149 g006
Table 1. Scintillation performance summary of common scintillators [5].
Table 1. Scintillation performance summary of common scintillators [5].
CrystalEx
(nm)
Em
(nm)
Decay Time
(ns)
Light Yield
(ph/MeV)
Normalized
to LYSO
Light Yield in 1st ns (Ph/MeV)
LYSO/LSO3584024030,000100740
CsI(TI)322540110060,00020055
NaI(TI)34641023036,000120160
Ce:GAGG4305505334,400115640
Ce:LuAG4505205025,00083240
Ce:YAG4605207021,00070130
BaF2X-ray220&3000.5&60013,000431200
Ce:YAP3003703412,00040390
BGO30448030080002727
Sapphire:Ti50075032007900262.5
CeF32653013026008.785
Y:BaF2X-ray220&3000.5&60020006.71200
AFO glass335365384501.512
PWO310420&42510&301300.436
Yb:YAG2603502.51100.3736
Yb:YAP2603501.1570.1934
Table 2. SCFs sample characteristics, energy resolution and fluorescence lifetime with different Ce dopant concentrations.
Table 2. SCFs sample characteristics, energy resolution and fluorescence lifetime with different Ce dopant concentrations.
SCFsGrowth Speed
mm/h
AnnealingPeakFWHMEnergy Resolution
[%]
Fluorescence Lifetime
ns
1 at% Ce:LuAG8No187.6424.7513.1956.35
1 at% Ce:LuAG8Yes211.732.6715.4356.95
0.3 at% Ce:LuAG8No169.3222.8213.4856.16
0.3 at% Ce:LuAG8Yes209.4429.9014.2855.73
0.3 at% Ce:LuAG16No169.8819.4111.4356.25
0.3 at% Ce:LuAG16Yes208.5131.4915.1057.14
0.1 at% Ce:LuAG8No175.8226.4315.0355.31
0.1 at% Ce:LuAG8Yes207.1833.3316.0854.87
0.1 at% Ce:LuAG16No190.6724.5112.8555.31
0.1 at% Ce:LuAG16Yes200.9530.4615.1654.58
Table 3. Comparison of performance of Ce:LuAG grown by different growth methods.
Table 3. Comparison of performance of Ce:LuAG grown by different growth methods.
MethodCe Concentration (%)Growth Speed
mm/h
Energy Resolution
[%]
Fluorescence Lifetime
[ns]
Ref
μ-PD0.130//[3]
CZ0.251/48[32]
transparent
ceramics
0.3/15.658[31]
This work0.34511.456/
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Dai, Y.; Zhang, Z.; Wang, X.; Lu, Z.; Kou, H.; Su, L.; Wu, A. Growth and Characterization of Ce-Doped Luag Single Crystal Fibers from Transparent Ceramics by Laser-Heated Pedestal Method. Crystals 2021, 11, 1149. https://0-doi-org.brum.beds.ac.uk/10.3390/cryst11091149

AMA Style

Dai Y, Zhang Z, Wang X, Lu Z, Kou H, Su L, Wu A. Growth and Characterization of Ce-Doped Luag Single Crystal Fibers from Transparent Ceramics by Laser-Heated Pedestal Method. Crystals. 2021; 11(9):1149. https://0-doi-org.brum.beds.ac.uk/10.3390/cryst11091149

Chicago/Turabian Style

Dai, Yun, Zhonghan Zhang, Xibin Wang, Zhuowei Lu, Huamin Kou, Liangbi Su, and Anhua Wu. 2021. "Growth and Characterization of Ce-Doped Luag Single Crystal Fibers from Transparent Ceramics by Laser-Heated Pedestal Method" Crystals 11, no. 9: 1149. https://0-doi-org.brum.beds.ac.uk/10.3390/cryst11091149

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop