Article

Precise Confinement and Position Distribution of Atomic Cu and Zn in ZSM-5 for CO2 Hydrogenation to Methanol

Shanghai Key Laboratory of Molecular Catalysis and Innovative Materials, Department of Chemistry, Fudan University, Shanghai 200438, China
*
Authors to whom correspondence should be addressed.
Nanomaterials 2023, 13(23), 3053; https://0-doi-org.brum.beds.ac.uk/10.3390/nano13233053
Submission received: 9 November 2023 / Revised: 27 November 2023 / Accepted: 28 November 2023 / Published: 29 November 2023
(This article belongs to the Section Physical Chemistry at Nanoscale)

Abstract

:
CuZn-based catalysts are widely used in CO2 hydrogenation, which may effectively convert CO2 to methanol and alleviate CO2 emission issues. The precise design of a model catalyst with a clear atomic structure is crucial in studying the relationship between structure and catalytic activity. In this work, a one-pot strategy was used to synthesize CuZn@ZSM-5 catalysts with approximately two Cu atoms and one Zn atom per unit cell. Atomic Cu and Zn species are confirmed to be located in the [54.6.102] and [62.104] tilings, respectively, by using magic-angle spinning nuclear magnetic resonance spectroscopy (MAS NMR), synchrotron X-ray powder diffraction (SXRD) and high-signal-to-noise-ratio annular dark field scanning transmission electron microscopy (High SNR ADF-STEM). Catalytic hydrogenation of CO2 to methanol was used as a model reaction to investigate the activity of the catalyst with confined active species. Compared to the Cu@ZSM-5, Zn@ZSM-5 and their mixture, the CuZn@ZSM-5 catalyst with a close Cu–Zn distance of 4.5 Å achieves a comparable methanol space–time yield (STY) of 92.0 mgmethanol·gcatal−1·h−1 at 533 K and 4 MPa with high stability. This method is able to confine one to three metal atoms in the zeolite channel and avoid migration and agglomeration of the atoms during the reaction, which maintains the stability of the catalyst and provides an efficient way for adjustment of the type and number of metal atoms along with the distances between them in zeolites.

1. Introduction

The environmental problems caused by greenhouse gas CO2 emissions are becoming increasingly imminent [1]. Capturing and separating CO2 from concentrated emission sources and using it as a C1 chemical raw material to produce methanol, formic acid, dimethyl ether and other chemicals has aroused widespread research interest [2,3,4,5]. Methanol can be used as a clean fuel or as a key chemical used to synthesize high-value-added derivatives with broad industrial prospects. Currently, the industrial process for preparing methanol is normally based on syngas as the raw material, which has been developed since 1961 [6]. With the increased importance of CO2 emission reduction and the shortage of petroleum resources, the CO and CO2 hydrogenation to methanol reaction is receiving more attention [7,8].
The synthesis of methanol from syngas or CO2 hydrogenation commonly uses Cu–ZnO–Al2O3 as a catalyst, where the Al2O3 is used to support the active Cu and Zn species [9]. Whether the active sites of CO2 hydrogenation to methanol reactions are Cu–ZnO interfacial sites or Cu–Zn alloy sites remains controversial [10,11,12]. However, the coexistence of Cu, Cu–Zn alloy and ZnO phases in catalysts prepared by impregnation or co-precipitation methods is inevitable, which causes great difficulties in the study of the relationship between the structure of catalysts and their activity [13]. In addition, due to the increase in surface energy of metal species with decreasing particle size, metal species dispersed on supports are thermodynamically unstable and prone to sintering during reaction [14]. The above factors may significantly reduce the metal dispersion and lead to rapid deactivation, limiting their practical industrial application [15]. The introduction of the confinement effect in the preparation of catalysts not only improves the regulation of catalytic active sites but also enhances phase purity and structural stability [16]. This confinement effect may be achieved by separating active metal species using zeolites [17,18,19,20,21,22], metal–organic frameworks [23,24] and two-dimensional layered materials [25] with their special porous structures, leading to the anti-sintering performance of catalysts and stability enhancement [26,27,28].
Zeolites are widely used in heterogeneous catalysis due to their unique microporous framework structures and high stability [29]. In ZSM-5, eight 5-membered ring [58] tilings with D2d symmetry construct characteristic two-dimensional 10-membered ring (10MR) channels. The 10MR channels parallel to the a-axis direction are zigzagged with a pore size of 5.5 Å × 5.1 Å, and the 10MR channels parallel to the b-axis direction are straight with a pore size of 5.3 Å × 5.6 Å [30,31,32]. These channels with moderate size provide the possibility for the confinement of metals. The one-pot synthesis strategy has been used to confine metal atoms in zeolites, such as Cu-CHA [33,34], Cu@FAU [28], Pt@Silicalite-1 [20], Pt@Ge-UTL [27], etc. STEM [26], EXAFS [27] and SXRD [28] have been employed for the study of the precise position of metal atoms and metal–metal or metal–framework interactions. These efforts show that the controllable synthesis and characterization of catalysts, especially the precise positioning of metal atoms, are particularly important for studying the structure–activity relationship of catalysts.
In this work, a series of M@ZSM-5 catalysts (M represents Cu, Zn, CuZn) were prepared by a one-pot synthesis method. The metals with close distances were located in specific positions in the zeolite channels using MAS NMR, SXRD and High SNR ADF-STEM techniques. The catalytic activity of Cu and Zn in M@ZSM-5 catalysts was investigated in CO2 hydrogenation to methanol reactions. The synergistic effect of different mixing modes for M@ZSM-5 catalysts on the catalytic activity was also studied.

2. Materials and Methods

2.1. Materials

Sodium aluminate (Al2O3 = 52.82%, Na2O = 40.24%, Alfa Aesar, Waltham, MA, USA), tetraethylorthosilicate (TEOS, SiO2 = 28%, Cross, Houston, TX, USA), sodium hydroxide (NaOH, ≥98%, Greagent, Shanghai, China), copper nitrate trihydrate (Cu(NO3)2·3H2O, 99%, Sinopharm, Shanghai, China) and zinc nitrate hexahydrate (Zn(NO3)2·6H2O, 99%, Sinopharm) were used as Al, Si, Na, Cu and Zn sources, respectively, while tetrapropylammonium hydroxide aqueous solution (TPAOH, 40 wt.%, Energy chemical, Shanghai, China) was employed as a structure-directing agent along with ethylenediamine (EDA, 99%, Sinopharm, Shanghai, China). All the reagents were used without further purification.

2.2. Catalyst Synthesis

ZSM-5 samples were obtained using a hydrothermal method with a composition of 0.5 Al2O3:100 SiO2:20 TPAOH:4 Na2O:2500 H2O [35]. In a typical synthesis, 0.13 g of NaOH and 19.45 g of deionized water were weighed in a 100 mL beaker in sequence, 0.05 g of sodium aluminate and 5.08 g of TPAOH were added with stirring, and then 10.71 g of TEOS was added to this solution and stirred for more than 4 h. The final gel was transferred to a 100 mL Teflon-lined autoclave, heated at a rate of 2 K·min−1 to 443 K, kept at this temperature for 72 h, and cooled naturally to room temperature. The product was separated by centrifugation and washed with deionized water and ethanol. Finally, the powder sample was calcined in a muffle furnace at 823 K for 6 h.
The compositions for Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 were 0.5 Al2O3:100 SiO2:20 TPAOH:4 Na2O:2500 H2O:2 Cu(NO3)2:4 EDA, 0.5 Al2O3:100 SiO2:20 TPAOH:4 Na2O:2500 H2O:1 Zn(NO3)2:3 EDA and 0.5 Al2O3:100 SiO2:20 TPAOH:4 Na2O:2500 H2O:2 Cu(NO3)2:1 Zn(NO3)2:7 EDA, respectively. An amount of 0.24 g of Cu(NO3)2·3H2O or/and 0.10 g of Zn(NO3)2·6H2O were weighed in a 50 mL beaker, and 5 g of deionized water was added. A transparent solution was formed after a desired amount of EDA was slowly added. The solution was then added dropwise to the above gel for the synthesis of ZSM-5 and finally TEOS was added. The remaining procedures were the same as that for the synthesis of ZSM-5 [20,35].

2.3. Characterization Techniques

X-ray diffraction (XRD) patterns were recorded on a Bruker D2 PHASER Advance diffractometer (Brucker, Madison, WI, USA), operated at 30 kV and 10 mA using Cu Kα (λ = 1.5418 Å) with a step width of 0.01° and a step time of 0.2 s. High-resolution SXRD data were obtained from MYTHEN detectors on a BL02B2 SPring-8 Japan [36] and refined by the Rietveld method using TOPAS refinement software (TOPAS-Academic V7). The patterns were collected in the 2θ range of 2–80° with 0.006° steps. Each pattern was collected for 4 min. In total, there were more than 800 hkl reflections measured, of which at least 300 independent hkl reflections were observed.
High SNR ADF-STEM images were captured on a JEM-ARM300F GRAND ARM (JEOL, Tokyo, Japan) aberration-corrected scanning transmission electron microscope equipped with double aberration correctors with an operating voltage of 300 kV and camera length of 800 mm. Image acquisition according to methods reported in the literature was conducted with a semi-angle of 10 mard, collection angles of 10–40 mard and an electron dose of 2653 e2 [37]. High-resolution transmission electron microscope photographs (HR-TEM) were obtained and selected-area electron diffraction (SAED) and elemental analysis (EDX) were performed using the Tecnai G2 F20 S-Twin (FEI, Hillsboro, OR, USA) field emission transmission electron microscope operated at 200 kV and equipped with an Oxford Instruments X-Max 80T EDS (Oxford Instruments, Abingdon, Oxfordshire, UK) probe.
Solid-state MAS NMR experiments were recorded using a Bruker AVANCE III 400WB NMR spectroscope (Brucker, Madison, WI, USA) at 9.4 T equipped with BL4 and BL7 MAS DVT probes (Brucker, Madison, WI, USA) using zirconia rotors with Kel-F caps. 27Al MAS NMR spectra were obtained at 104.3 MHz using a 4 mm rotor with a spinning rate of 12 kHz. A single-pulse sequence was used with a 10° pulse (0.13 μs) and a recycle delay of 0.3 s. The powder zeolite samples were balanced at the desired humidity in a glass container over a saturated MgCl2 aqueous solution for more than 24 h prior to 27Al NMR measurements. 29Si MAS NMR spectra were obtained at 79.6 MHz using a 7 mm rotor with a spinning rate of 4 kHz. A single-pulse sequence was used with a 90° pulse (4.3 μs) and a recycle delay of 180 s. 1H-29Si CP/MAS NMR spectra were recorded with a 90° pulse (4.3 μs), a contact time of 1–18 ms and a recycle delay of 2 s. A 1 M Al(NO3)3 aqueous solution and tetramethylsilane (Si(CH3)4, TMS) were used as the 27Al and 29Si external chemical shift standards, respectively.
X-ray photoelectron spectroscopy (XPS) was performed using a PHI PHI5000C instrument equipped with a Versa probe and a Mg Kα emission light source (hv = 1253.6 eV) at 15 kV and 20 mA. Binding energy was calibrated with the contaminated carbon C 1s of 284.8 eV.
A N2 adsorption–desorption study was carried out on a Micromeritics ASAP 2020 Plus analyzer (Micromeritics, Norcross, GA, USA) at 77 K. The samples were pretreated at 573 K and 1.3 × 10−2 Pa for 10 h. The specific surface area was obtained using the Brunauer–Emmett–Teller (BET) equation and the micropore volume and micropore surface areas were calculated using a t-plot, and the pore size distribution was calculated using the Barrett–Joyner–Halenda model.
H2 temperature-programmed reduction (H2-TPR) was conducted using a Micromeritics ChemiSorb 2720 chemical adsorption instrument (Micromeritics, Norcross, GA, USA) with a thermal conductivity detector (TCD). A typical procedure was as follows: 100 mg of sample was loaded into a quartz U-tube and pretreated with He at 50 mL·min−1. The temperature was raised at a rate of 10 K·min−1 from ambient temperature to 473 K and maintained for 1 h and then lowered to below 317 K. The gas was switched to 10% H2/Ar and the temperature was raised at a rate of 10 K·min−1 to 923 K. Inductively coupled plasma atomic emission spectroscopy (ICP-AES) was performed using a Varian 725-ES plasma emission spectrometer.

2.4. Catalytic Tests

A stainless-steel reactor was equipped with a quartz tube liner with an inner diameter of 8 m and a length of 58 cm. A total of 0.1 g of 40–60 mesh catalyst was loaded with a layer height of about 0.5 cm. The reaction was carried out within the temperature range of 513–593 K, at a pressure of 4.0 MPa, a reaction gas composition H2/CO2/Ar of 72/24/4, a reaction gas flow rate of 40 mL·min−1 and a space velocity GHSV of 24,000 mL·gcatal−1·h−1.
A Huaai GC-9560 gas chromatograph (Shanghai Huaai Chromatographic Analysis Technology Co., Ltd., Shanghai, China) was equipped with a TCD and a flame ion detector (FID) for the analysis of products. CO2, CO, Ar, CH4 and some other products were analyzed with the TCD through a Porapak N-filled column (5 m × 2 mm) and a 13X zeolite-filled column (3 m × 2 mm). Light olefins and methanol were analyzed with the FID through an HP-PLOT Al2O3 capillary column (50 m × 0.32 mm × 10 μm). The conversion of CO2, the selectivity of products, the space–time yield (STY) of methanol and the apparent turnover frequency (TOF) for methanol were calculated as follows:
Conv .   CO 2   ( % ) = n CO 2 - in     n CO 2 - out n CO 2 in   ×   100 %
Select .   C i H j O k   ( % ) = i   ×   n C i H j O k i   ×   n C i H j O k   ×   100 %
STY methanol = GHSV   ×   Conv .   ×   Select .   ×   32   ×   0.24 22.4   ( mg methanol · g catal 1 · h 1 )
TOF methanol = GHSV   ×   Conv .   ×   Select .   ×   0.24 22.4   ×   1000   ×   ( Cu   wt . % 64 + Zn   wt . % 65 )   ( h 1 )

3. Results

3.1. Structural Characterization

The XRD patterns show that all ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 synthesized by the hydrothermal method have typical MFI structure (JCPDS No. 42-0023) without any impurity (Figure 1). No diffraction peaks assigned to Cu or Zn or their oxides are observed.
The morphology and structure of the synthesized zeolites were studied by TEM. Figure 2 shows the TEM, HRTEM and SAED images of the synthesized ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5. All samples exhibit a hexagonal prism with a short b axis. The average particle size and thickness along the b axis of ZSM-5, Cu@ZSM-5, Zn@ZSM-5, and CuZn@ZSM-5 are about 1 μm and 200 nm, 650 nm and 150 nm, 1.2 μm and 400 nm, and 200 nm and 80 nm, respectively. All samples are uniform in shape and size. From the HETEM images (Figure 2b,e,h,k), lattice fringes along the direction of [010] may be observed in all samples. Combined with the corresponding SAED images (Figure 2c,f,i,l), the lattice spacings of 10.01 and 11.13 Å correspond to the interplanar spacings of (200) and (101), respectively, and the angle between (200) and (101) planes is 56° [38].
The EDS mapping results (Figure S1) show that all elements in the samples are evenly distributed and no large-scale aggregation of Cu or Zn is observed. This indicates that Cu and Zn are well dispersed in zeolite framework or channels. The composition of the samples was determined by ICP-AES. The Si/Al ratio of ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 are 86, 79, 82 and 75, respectively, which are close to the Si/Al of 100 in the starting synthesis gel. The contents of metals in the samples are shown in Table 1 and are close to those in the starting synthesis gel.
Table 2 shows texture data of the products after calcination at 823 K for the removal of template molecules in the channels as part of the N2 adsorption–desorption experiments. All samples have typical microporous structures with the largest microporous specific surface area of 337 m2·g−1 found in ZSM-5. After introducing the metal species, the microporous specific surface areas decrease significantly and the smallest microporous specific surface area of CuZn@ZSM-5 is 193 m2·g−1. ZSM-5 has the maximum microporous volume of 0.13 cm3·g−1 among the four samples when compared with Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 which decrease by 0.03, 0.01 and 0.06 cm3·g−1, respectively. The MFI structural units form 10MR with a pore size of about 5.1–5.6 Å and 5MR with a size of about 2.6–3.1 Å. Since the kinetic diameter of N2 molecules is 3.04 Å, N2 adsorption can only detect the 10MR channels within the framework [39]. Through the trend change of microporous specific surface area and volume, it can be speculated that the confined metal Cu or/and Zn are located in the 10MR channel of the MFI framework. The confined metal species located in the microporous channels of the zeolite occupy part of the microporous space, affecting the adsorption of N2 molecules in the microporous channels and leading to a decrease in microporous volume and specific surface area.
The zeolite framework structure was further studied by MAS NMR. Figure 3 shows that the 27Al MAS NMR spectra of all samples have a sharp peak at 55 ppm, attributed to the four-coordinate framework aluminum. No peak is found at 0 ppm, indicating that the samples do not contain six-coordinate extra-framework aluminum [40].
Figure 4 and Figure 5 show the 29Si MAS NMR and 1H-29Si CP/MAS NMR spectra of ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5. In the 29Si MAS NMR spectra, all zeolites show four peaks located at −101, −105, −112 and −116 ppm. The peak at −101 ppm can be attributed to Q3 (Si(OSi)3(OAl)1 or Si(OSi)3OH), the peak at −105 ppm can be attributed to Q3 (Si(OSi)3(OAl)1), and the peaks at −112 and −116 ppm can be attributed to Q4 (Si(OSi)4) [41]. However, in the 1H-29Si CP/MAS NMR spectra, no NMR peak appears in the chemical shift range of −80~−120 ppm, indicating that the MFI framework has no hydroxyl defects and is intact after calcination. Therefore, the peak at −101 ppm in Figure 4 can be attributed to Si(OSi)3(OAl)1 rather than Si(OSi)3OH [42]. Since there are no amorphous Si species and strong XRD diffraction peaks, the synthesized products have high crystallinity. By fitting the peaks of each spectrum in Figure 4, Si/Al may be calculated and is listed in Table 3, which is basically consistent with the ICP-AES results.

3.2. Insight into the Confined Position of the Metal in ZSM-5

Since NMR results reflect the local environment of the Si atoms, different local environments of Si, particularly affected by metal introduced in the zeolite framework, may lead to a change in full-width-at-half-maximum (FWHM) even with the same Si/Al ratio. The deconvolution results of the 29Si MAS NMR spectra for ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 samples indicate similar FWHM for their corresponding peaks. Therefore, no heteroatom is introduced into the MFI framework [43]. In addition, if heteroatoms Cu or/and Zn are introduced into the MFI framework, the MFI framework forms defects, leading to the formation Si(OSi)3OH. This structural change may cause cross-polarization from H to Si, thus enhancing 1H-29Si CP/MAS NMR intensities. As seen in Figure 5, there is no 1H-29Si CP/MAS NMR peak in the range of −80~−120 ppm, indicating that there is no Si(OSi)3OH in the MFI framework after calcination and no heteroatoms have been introduced into the MFI framework.
To further study the structural relationship between the MFI framework and the introduced Cu or/and Zn species, a series of variable contact-time 1H-29Si CP/MAS NMR experiments were employed using the as-prepared (uncalcined) ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 samples. As shown in Figures S2–S5, the intensities of all peaks at −101, −105, −112 and −116 ppm reach a maximum at certain contact times, among which the peak at −112 ppm is the strongest and its intensity change with contact time is displayed in Figure 6. The contact times at the highest peak intensity for ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 are 12, 8, 10 and 6 ms, respectively. Although there is no heteroatom introduced into the MFI framework to form Si(OSi)3OH, the structure-directing agent containing H atoms in the zeolite channels may enhance the 1H-29Si cross-polarization. In addition, the existence of confined Cu or/and Zn in the channels may further reduce the motion of H atoms and the distance between H and Si, thus reducing the optimal CP contact time [44,45,46], which is consistent with the results shown in Figure 6. Therefore, the various contact-time 1H-29Si CP/MAS NMR experiments clearly show the confinement of Cu or/and Zn in the ZSM-5 channels.
In order to have a better understanding of the location of the confined metals in the zeolite structure at the atomic level, synchrotron X-ray diffraction was carried out to obtain SXRD patterns (Figure 7) for the samples of Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 [36]. The refined structures of the samples were obtained by the Rietveld method using TOPAS software (TOPAS-Academic V7), and the fitted crystallographic parameters are shown in Table S1, and atomic information from the Rietveld refinement of the samples are listed in Tables S2–S4. According to the fitting results, it can be seen that the Rwp of Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 are 7.59%, 9.23% and 9.69%, respectively, indicating the high credibility of the fitting results [47]. The inset patterns in Figure 7 show that the error line fluctuates slightly in the 2θ range of 20–40°, reflecting the high quality and accuracy of refining local structures [39]. Combined with the ICP-AES results, the average contents of Cu, Zn and CuZn per unit cell of Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 are 1.82, 0.88 and 2.34/0.89, respectively.
Based on the refined structures (Tables S2–S4), the positional relationship between the confined metal atoms and the MFI framework in Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 are shown in Figure 8. According to the probability distribution of confined metal from the structural model obtained by SXRD analysis, there are two different positions of Cu in the Cu@ZSM-5 sample. Cu-1 is located in the [54.6.102] tiling (Figure 8a), and the shortest Cu–O distance between Cu-1 and the surrounding framework structure is 3.9 Å. Cu-2 is located in the [62.104] tiling (Figure 8b), and the shortest Cu–O distance between Cu-2 and the surrounding framework structure is 2.7 Å. The ratio of Cu-1 to Cu-2 is 1.20. Zn in the Zn@ZSM-5 is located in the [54.6.102] tiling (Figure 8c), and the shortest Zn–O distance to the surrounding framework structure is 3.3 Å. There are two types of Cu atoms and one type of Zn atom in the CuZn@ZSM-5 sample. Both Cu atoms are located in the unit composed of the [62.104] tiling (Figure 8d). The distance between two Cu atoms is 5.2 Å. Zn is located in the unit composed of the [54.6.102] tiling (Figure 8e). The distance between Cu and Zn is 4.5–5.5 Å. The positions of the [54.6.102] tiling and the [62.104] tiling in the MFI framework are shown in Figure 8f, where the [54.6.102] tiling is part of the sinusoidal channel, and the [62.104] tiling is located at the intersection of the sinusoidal channel and the straight channel. Based on the above SXRD results, combined with the N2 adsorption and 1H-29Si CP/MAS NMR results, it can be concluded that Cu and Zn species are confined in zeolite channels without entering the framework as heteroatoms.
Figure 9 shows the High SNR ADF-STEM results for CuZn@ZSM-5. The atomic -resolution image and intensity analysis provides actual spatial evidence of the zeolite framework with metal atoms in the channels [26,37]. The metal atoms in the channels of the MFI framework are directly visualized along the [010] zone axis as Figure 9a. Among them, position 1# is an empty channel, and the diameter of the hole is 5–6 Å which is consistent with the size of the 10MR of the MFI framework. The metal atoms in positions 2# and 3# can be identified by Z-contrast with an atomic radius of less than 2 Å and the distance between metal atoms and the framework is about 3–4 Å as shown in Figure 9b,c. This implies that the metal atoms occupy specific positions in the MFI channels, which is consistent with the confinement of metals mentioned above in SXRD and MAS NMR.
The valence states of the confined metals Cu and Zn were studied using XPS. Figure 10 shows the XPS spectra of Cu 2p and Zn 2p for Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 and their relevant results are shown in Table 4. The appearance of the satellite peak at 945.3 eV in the Cu 2p XPS of Cu@ZSM-5 and CuZn@ZSM-5 indicates the presence of Cu2+ ions. The Cu 2p3/2 has two peaks at 933.7 and 935.3 eV and Cu 2p1/2 at 953.7 and 956.0 eV, which are attributed to two different Cu2+ ions located in different tilings (Table S5) [48]. The area ratio of the XPS peak for Cu-2:Cu-1 in Cu@ZSM-5 is 1.25, which is close to that of the SXRD result for Cu-2:Cu-1 of 1.20. In the CuZn@ZSM-5 sample, the XPS result shows only one type of Cu. Combined with the SXRD results, two Cu2+ ions are located in the [62.104] tiling and the chemical environments of them are same. The binding energies of Zn 2p3/2 and 2p1/2 are 1022.4 and 1045.8 eV, respectively, attributed to Zn2+ (Table S5) [49].
H2-TPR (Figure S6) shows that a reduction peak appears near 505 K for Cu@ZSM-5 and CuZn@ZSM-5, which can be attributed to the reduction peak of Cu2+ [9]. No obvious peak related to the reduction of Zn2+ may be observed in Zn@ZSM-5 and CuZn@ZSM-5, indicating that Zn2+ is not able to be reduced below 900 K. Since there is no change in the Cu2+ and Zn2+ reduction temperatures, it indicates that there is no interaction between Cu2+ and Zn2+, which further proves that Cu2+ and Zn2+ are located in different MFI channels.

3.3. Catalytic Performance

CO2 hydrogenation to methanol was investigated as a model reaction under a pressure of 4.0 MPa, a H2/CO2/Ar composition of 72/24/4 and a GHSV of 24,000 mL·gcatal−1·h−1 with a temperature range of 513–593 K. Figure 11a,b shows the results of CO2 hydrogenation to methanol with Cu@ZSM-5 and Zn@ZSM-5 at different temperatures. With an increase in reaction temperature from 513 K to 593 K, the CO2 conversion over the Cu@ZSM-5 catalyst increases from 2.48% to 23.6%, with a high CO selectivity of >96%. As reported by Kattel et al., Cu species can dissociate H2 rapidly, weaken CO* binding and hinder CO* hydrogenation within the temperature range of 525–575 K [11]; therefore, CO becomes the main product [50]. From 513 to 593 K, the CO2 conversion over the Zn@ZSM-5 catalyst is less than 3% with the methanol selectivity decreasing from 66% to 47%. Compared with Cu species, the higher oxophilicity of Zn in Zn@ZSM-5 promotes the hydrogenation of oxygenated intermediates to methanol [51,52]. With an increase in reaction temperature, the reverse water gas shift reaction intensifies, leading to a gradual increase in CO selectivity [53].
The influence of CuZn bimetallic coupling on CO2 hydrogenation was studied with three mixing methods: (1) CuZn@ZSM-5 catalyst with bimetallic confinement (Figure 11c), (2) Cu@ZSM-5 particles mixed with Zn@ZSM-5 particles (Figure 11d) and (3) dual bed of Cu@ZSM-5 followed by Zn@ZSM-5 (Figure 11e). The distances between Cu and Zn in the above methods (1)–(3) are <1 nm, 200–400 μm and 0.5–1 cm, respectively. As the reaction temperature increases, over the catalysts in all three systems, the conversions of CO2 increase and the selectivity to methanol decreases, and the selectivity to byproduct CO increases. At 533 K, the methanol STY over CuZn@ZSM-5 reaches 92.0 mgmethanol·gcatal·h−1 with a selectivity to methanol of 66.6% and a TOF for methanol of 5.90 h−1, while over the catalysts as described in methods (2) and (3), the methanol STY values are 9.92 and 6.38 mgmethanol·gcatal−1·h−1 (Figure 11f), the selectivity to methanol values are 4.04% and 1.91%, and the TOF values of methanol are 1.46 and 0.935 h−1, respectively. The main product for physically mixed particles with a Cu–Zn distance of 200–400 μm or dual beds with a distance of 0.5–1 cm of Cu@ZSM-5 and Zn@ZSM-5 is CO, which is similar to that of Cu@ZSM-5. Only when Cu and Zn species are in a close proximity in CuZn@ZSM-5 (<1 nm) does methanol becomes dominant in the main products along with the increase in CO2 conversion due to the synergistic effect of Cu and Zn species [54]. Therefore, it is expected that the close distance between Cu and Zn in CuZn@ZSM-5 may play a key role in high selective methanol formation. As the design of catalysts with confinement effects at atomic and sub-nanometer scales is still not mature, it can be further optimized by adjusting the type, distance and number of confined metals.
In addition to CO and methane, water is also a byproduct of the CO2 hydrogenation to methanol reaction. Under high-temperature and high-pressure conditions, the presence of water is detrimental to the stability of the zeolite framework, resulting in the removal of framework aluminum and the formation of framework defects affecting the stability of the catalyst. Figure S9 shows the XRD patterns of the CuZn@ZSM-5 catalyst before and after use for 50 h, indicating that the MFI framework remains stable. In addition, the 27Al MAS NMR spectra in Figure S10 further prove that there is no aluminum removed from the MFI framework during the reaction. In Figure S11a, lattice stripes with spacings of 10.01 Å and 11.13 Å and an angle of 56° between them are observed, spacings of 10.01 Å and 11.13 Å represent reflecting the (200) and (101) planes and the incident direction of [010], respectively. HAADF-STEM imagery (Figure S11b) shows that no obvious large metal clusters exist in the channels and the MFI framework structure is intact. EDS (Figure S11c) can only find well-dispersed Cu, Zn and Al elements within the MFI framework, and no agglomerate is observed. The Cu and Zn confined within the channels exhibit high stability.

4. Conclusions

A series of M@ZSM-5 catalysts (M represents Cu, Zn, CuZn) were prepared by a hydrothermal method. XRD, TEM and MAS NMR characterization show that the catalysts have high crystallinity without agglomerated metal particles, framework defects and extra-framework aluminum. The locations of confined metals were successfully determined by multiple characterization techniques. 1H-29Si CP/MAS NMR with variable contact time exhibit that the introduced metal species are confined in the zeolite channels with no framework of Cu and Zn species. The probability distribution structure models obtained by SXRD analysis prove that metal atoms are located at the intersection of straight and sinusoidal channels or in the sinusoidal channel of the MFI structure in M@ZSM-5 catalysts. Metal atoms in pore channels were directly observed in High SNR ADF-STEM images. This synthetic method may pave a way to fabricating stable catalysts with a single or several metal atoms in zeolite channels. In the model CO2 hydrogenation to methanol reaction, the CuZn@ZSM-5 catalyst with a sub-nanometer Cu–Zn distance achieves a maximum methanol STY of 92.0 mgmethanol·gcatal−1·h−1 at 533 K and 4 MPa. The MFI structure of CuZn@ZSM-5 remains almost constant without metal agglomeration contributed by the confinement effect of the zeolite channels after a 50 h reaction.

Supplementary Materials

The following supporting information can be downloaded at: https://0-www-mdpi-com.brum.beds.ac.uk/article/10.3390/nano13233053/s1, Figure S1. EDS Mapping of (a) ZSM-5, (b) Cu@ZSM-5, (c) Zn@ZSM-5 and (d) CuZn@ZSM-5; Figure S2. 1H-29Si CP/MAS NMR spectra of ZSM-5 at different contact time before calcination; Figure S3. 1H-29Si CP/MAS NMR spectra of Cu@ZSM-5 at different contact time before calcination; Figure S4. 1H-29Si CP/MAS NMR spectra of Zn@ZSM-5 at different contact time before calcination; Figure S5. 1H-29Si CP/MAS NMR spectra of CuZn@ZSM-5 at different contact time before calcination; Figure S6. H2-TPR curves of (a) ZSM-5, (b) Cu@ZSM-5, (c) Zn@ZSM-5 and (d) CuZn@ZSM-5; Figure S7. XRD patterns of CuZn@ZSM-5 catalyst before and after 50 h reaction; Figure S8. 27Al MAS NMR spectra of CuZn@ZSM-5 catalyst before and after 50 h reaction; Figure S9. (a) HRTEM and SAED (inset), (b) HAADF-STEM and (c) EDS of CuZn@ZSM-5 after 50 h reaction; Table S1: Crystallographic and TOPAS fitting parameters. Table S2. Atomic information from the Rietveld refinement of Cu@ZSM-5. Table S3. Atomic information from the Rietveld refinement of Zn@ZSM-5. Table S4. Atomic information from the Rietveld refinement of CuZn@ZSM-5. Table S5. Binding energy of Cu 2p3/2 and Zn 2p3/2 [48,49].

Author Contributions

H.D.: data acquisition, analysis and interpretation and writing—original draft; J.Z., W.F. and Q.Y.: formal analysis and discussion; L.Z. and Y.R.: formal analysis, visualization; L.Y., B.Y. and H.H.: conception and design, validation, writing—review and editing, supervision. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by the National Natural Science Foundation of China (22088101) and the Ministry of Science and Technology (2022YFA1503504 and 2022YFA1503802).

Data Availability Statement

Data will be made available on request.

Acknowledgments

The authors thank WANG Lingling (JEOL) for their help in the High SNR ADF-STEM measurements and data interpretations.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Zhang, Q.; Yu, J.H.; Corma, A. Applications of zeolites to C1 chemistry: Recent advances, challenges, and opportunities. Adv. Mater. 2020, 32, 2002927. [Google Scholar] [CrossRef] [PubMed]
  2. Cui, X.J.; Huang, R.; Deng, D.H. Catalytic conversion of C1 molecules under mild conditions. EnergyChem 2021, 3, 100050. [Google Scholar] [CrossRef]
  3. Zhou, W.; Cheng, K.; Kang, J.C.; Zhou, C.; Subramanian, V.; Zhang, Q.H.; Wang, Y. New horizon in C1 chemistry: Breaking the selectivity limitation in transformation of syngas and hydrogenation of CO2 into hydrocarbon chemicals and fuels. Chem. Soc. Rev. 2019, 48, 3193–3228. [Google Scholar] [CrossRef]
  4. Bhattacharyya, S.S.; Leite, F.F.G.D.; Adeyemi, M.A.; Sarker, A.J.; Cambareri, G.S.; Faverin, C.; Tieri, M.P.; Castillo-Zacarías, C.; Melchor-Martínez, E.M.; Iqbal, H.M.N.; et al. A paradigm shift to CO2 sequestration to manage global warming—With the emphasis on developing countries. Sci. Total Environ. 2021, 790, 148169. [Google Scholar] [CrossRef] [PubMed]
  5. Liu, Y.T.; Deng, D.H.; Bao, X.H. Catalysis for Selected C1 Chemistry. Chem 2020, 6, 2497–2514. [Google Scholar] [CrossRef]
  6. Wang, W.; Wang, S.P.; Ma, X.B.; Gong, J.L. Recent advances in catalytic hydrogenation of carbon dioxide. Chem. Soc. Rev. 2011, 40, 3703–3727. [Google Scholar] [CrossRef]
  7. Norhasyima, R.S.; Mahlia, T.M.I. Advances in CO₂ utilization technology: A patent landscape review. J.CO2 Util. 2018, 26, 323–335. [Google Scholar] [CrossRef]
  8. Jiang, X.; Nie, X.W.; Guo, X.W.; Song, C.S.; Chen, J.G. Recent Advances in Carbon Dioxide Hydrogenation to Methanol via Heterogeneous Catalysis. Chem. Rev. 2020, 120, 7984–8034. [Google Scholar] [CrossRef]
  9. Qi, S.C.; Liu, X.Y.; Zhu, R.R.; Xue, D.M.; Liu, X.Q.; Sun, L.B. Causation of catalytic activity of Cu-ZnO for CO2 hydrogenation to methanol. Chem. Eng. J. 2022, 430, 132784. [Google Scholar] [CrossRef]
  10. Kuld, S.; Conradsen, C.; Moses, P.G.; Chorkendorff, I.; Sehested, J. Quantification of zinc atoms in a surface alloy on copper in an industrial-type methanol synthesis catalyst. Angew. Chem. Int. Ed. 2014, 53, 5941–5945. [Google Scholar] [CrossRef]
  11. Kattel, S.; Ramírez, P.J.; Chen, J.G.; Rodriguez, J.A.; Liu, P. Active sites for CO2 hydrogenation to methanol on Cu/ZnO catalysts. Science 2017, 355, 1296–1299. [Google Scholar] [CrossRef] [PubMed]
  12. Van Deelen, T.W.; Hernández Mejía, C.; de Jong, K.P. Control of metal-support interactions in heterogeneous catalysts to enhance activity and selectivity. Nat. Catal. 2019, 2, 955–970. [Google Scholar] [CrossRef]
  13. Hartley, U.W.; Murugesan, P.K. Chapter 12: Dual Functional Nano Zeolites for CO2 Capture and Conversion; Elsevier: Amsterdam, The Netherlands, 2023; pp. 309–332. [Google Scholar]
  14. Wang, H.; Wang, L.; Xiao, F.S. Metal@zeolite hybrid materials for catalysis. ACS Cent. Sci. 2020, 6, 1685–1697. [Google Scholar] [CrossRef]
  15. Zhang, F.Y.; Zhou, W.; Xiong, X.W.; Wang, Y.H.; Cheng, K.; Kang, J.C.; Zhang, Q.H.; Wang, Y. Selective hydrogenation of CO2 to ethanol over sodium-modified Rhodium nanoparticles embedded in zeolite Silicalite-1. J. Phys. Chem. C 2021, 125, 24429–24439. [Google Scholar] [CrossRef]
  16. Leung, K.C.; Hong, S.; Li, G.C.; Xing, Y.D.; Ng, B.K.Y.; Ho, P.L.; Ye, D.P.; Zhao, P.; Tan, E.; Safonova, O.; et al. Confined Ru sites in a 13X zeolite for ultrahigh H2 production from NH3 decomposition. J. Am. Chem. Soc. 2023, 145, 14548–14561. [Google Scholar] [CrossRef]
  17. Choi, M.; Wu, Z.J.; Iglesia, E. Mercaptosilane-assisted synthesis of metal clusters within zeolites and catalytic consequences of encapsulation. J. Am. Chem. Soc. 2010, 132, 9129–9137. [Google Scholar] [CrossRef]
  18. Goel, S.; Wu, Z.J.; Zones, S.I.; Iglesia, E. Synthesis and catalytic properties of metal clusters encapsulated within small-pore (SOD, GIS, ANA) zeolites. J. Am. Chem. Soc. 2012, 134, 17688–17695. [Google Scholar] [CrossRef]
  19. Goel, S.; Zones, S.I.; Iglesia, E. Encapsulation of metal clusters within MFI via interzeolite transformations and direct hydrothermal syntheses and catalytic consequences of their confinement. J. Am. Chem. Soc. 2014, 136, 15280–15290. [Google Scholar] [CrossRef] [PubMed]
  20. Wang, N.; Sun, Q.M.; Bai, R.S.; Li, X.; Guo, G.Q.; Yu, J.H. In situ confinement of ultrasmall Pd clusters within nanosized Silicalite-1 zeolite for highly efficient catalysis of hydrogen generation. J. Am. Chem. Soc. 2016, 138, 7484–7487. [Google Scholar] [CrossRef]
  21. Zhang, J.; Wang, L.; Shao, Y.; Wang, Y.Q.; Gates, B.C.; Xiao, F.S. A Pd@zeolite catalyst for nitroarene hydrogenation with high product selectivity by sterically controlled adsorption in the zeolite micropores. Angew. Chem. Int. Ed. 2017, 56, 9747–9751. [Google Scholar] [CrossRef]
  22. Zhang, J.; Wang, L.; Zhang, B.S.; Zhao, H.S.; Kolb, U.; Zhu, Y.H.; Liu, L.M.; Han, Y.; Wang, G.X.; Wang, C.T.; et al. Sinter-resistant metal nanoparticle catalysts achieved by immobilization within zeolite crystals via seed-directed growth. Nat. Catal. 2018, 1, 540–546. [Google Scholar] [CrossRef]
  23. Cui, W.G.; Zhang, Q.; Zhou, L.; Wei, Z.C.; Yu, L.; Dai, J.J.; Zhang, H.B.; Hu, T.L. Hybrid MOF template-directed construction of hollow-structured In2O3@ZrO2 heterostructure for enhancing hydrogenation of CO2 to methanol. Small 2022, 19, 2204914. [Google Scholar] [CrossRef] [PubMed]
  24. Li, Q.; Gao, Y.X.; Zhang, M.; Gao, H.; Chen, J.; Jia, H.P. Efficient infrared-light-driven photothermal CO2 reduction over MOF-derived defective Ni/TiO2. Appl. Catal. B 2022, 303, 120905. [Google Scholar] [CrossRef]
  25. Wang, Y.; Zhang, W.H.; Deng, D.H.; Bao, X.H. Two-dimensional materials confining single atoms for catalysis. Chin. J. Catal. 2017, 38, 1443–1453. [Google Scholar] [CrossRef]
  26. Tang, X.; Ye, J.J.; Guo, L.S.; Pu, T.C.; Cheng, L.; Cao, X.M.; Guo, Y.L.; Wang, L.; Guo, Y.; Zhan, W.C.; et al. Atomic Insights into the Cu Species Supported on Zeolite for Direct Oxidation of Methane to Methanol via Low-Damage HAADF-STEM. Adv. Mater. 2023, 35, 2208504. [Google Scholar] [CrossRef] [PubMed]
  27. Ma, Y.; Song, S.J.; Liu, C.C.; Liu, L.m.; Zhang, L.K.; Zhao, Y.H.; Wang, X.; Xu, H.; Guan, Y.J.; Jiang, J.A.; et al. Germanium-enriched double-four-membered-ring units inducing zeolite-confined subnanometric Pt clusters for efficient propane dehydrogenation. Nat. Catal. 2023, 6, 506–518. [Google Scholar] [CrossRef]
  28. Chai, Y.C.; Qin, B.; Li, B.N.; Dai, W.L.; Wu, G.J.; Guan, N.J.; Li, L.D. Zeolite-encaged mononuclear copper centers catalyze CO2 selective hydrogenation to methanol. Natl. Sci. Rev. 2023, 10, nwad043. [Google Scholar] [CrossRef]
  29. Shamzhy, M.; Opanasenko, M.; Concepción, P.; Martínez, A. New trends in tailoring active sites in zeolite-based catalysts. Chem. Soc. Rev. 2019, 48, 1095–1149. [Google Scholar] [CrossRef]
  30. Kokotailo, G.T.; Lawton, S.L.; Olson, D.H.; Meier, W.M. Structure of synthetic zeolite ZSM-5. Nature 1978, 272, 437–438. [Google Scholar] [CrossRef]
  31. Olson, D.H.; Kokotailo, G.T.; Lawton, S.L.; Meier, W.M. Crystal structure and structure-related properties of ZSM-5. J. Phys. Chem. 1981, 85, 2238–2243. [Google Scholar] [CrossRef]
  32. Van Koningsveld, H.; Jansen, J.C.; van Bekkum, H. The monoclinic framework structure of zeolite H-ZSM-5. Comparison with the orthorhombic framework of as-synthesized ZSM-5. Zeolites 1990, 10, 235–242. [Google Scholar] [CrossRef]
  33. Ren, L.M.; Zhu, L.F.; Yang, C.G.; Chen, Y.M.; Sun, Q.; Zhang, H.Y.; Li, C.J.; Nawaz, F.; Meng, X.J.; Xiao, F.S. Designed copper–amine complex as an efficient template for one-pot synthesis of Cu-SSZ-13 zeolite with excellent activity for selective catalytic reduction of NOx by NH3. Chem. Commun. 2011, 47, 9789–9791. [Google Scholar] [CrossRef]
  34. Wang, Y.Z.; Han, J.F.; Chen, M.Y.; Lv, W.T.; Meng, P.T.; Gao, W.; Meng, X.J.; Fan, W.B.; Xu, J.; Yan, W.F.; et al. Low-silica Cu-CHA zeolite enriched with Al Pairs transcribed from silicoaluminophosphate seed: Synthesis and ammonia selective catalytic reduction performance. Angew. Chem. Int. Ed. 2023, 62, e202306174. [Google Scholar] [CrossRef] [PubMed]
  35. Zhao, X.L.; Zeng, S.; Zhang, X.L.; Deng, Q.Z.; Li, X.J.; Yu, W.G.; Zhu, K.K.; Xu, S.T.; Liu, J.C.; Han, L. Generating assembled MFI nanocrystals with reduced b-axis through structure-directing agent exchange induced recrystallization. Angew. Chem. Int. Ed. 2021, 60, 13959–13968. [Google Scholar] [CrossRef]
  36. Kawaguchi, S.; Takemoto, M.; Osaka, K.; Nishibori, E.; Moriyoshi, C.; Kubota, Y.; Kuroiwa, Y.; Sugimoto, K. High-throughput powder diffraction measurement system consisting of multiple MYTHEN detectors at beamline BL02B2 of SPring-8. Rev. Sci. Instrum. 2017, 88, 085111. [Google Scholar] [CrossRef]
  37. Wang, L.L.; Jiang, Y.L.; Zhou, Y.; Shi, R.K.; Hosokawa, F.; Terasaki, O.; Zhang, Q. Improving Data Quality in Traditional Low-Dose Scanning Transmission Electron Microscopy Imaging. Part. Part. Syst. Charact. 2023, 40, 2200122. [Google Scholar] [CrossRef]
  38. Choudhary, M.K.; Kumar, M.; Rimer, J.D. Regulating nonclassical pathways of Silicalite-1 crystallization through controlled evolution of amorphous precursors. Angew. Chem. Int. Ed. 2019, 58, 15712–15716. [Google Scholar] [CrossRef]
  39. Choi, M.; Na, K.; Kim, J.; Sakamoto, Y.; Terasaki, O.; Ryoo, R. Stable single-unit-cell nanosheets of zeolite MFI as active and long-lived catalysts. Nature 2009, 461, 246–249. [Google Scholar] [CrossRef]
  40. Xin, S.H.; Wang, Q.; Xu, J.; Chu, Y.Y.; Wang, P.F.; Feng, N.D.; Qi, G.D.; Trébosc, J.; Lafon, O.; Fan, W.B.; et al. The acidic nature of “NMR-invisible” tri-coordinated framework aluminum species in zeolites. Chem. Sci. 2019, 10, 10159–10169. [Google Scholar] [CrossRef]
  41. Fyfe, C.A.; Brouwer, D.H. Effect of molecular oxygen on the variable-temperature 29Si MAS NMR spectra of zeolite−sorbate complexes. J. Am. Chem. Soc. 2004, 126, 1306–1307. [Google Scholar] [CrossRef]
  42. Christiansen, S.C.; Zhao, D.; Janicke, M.T.; Landry, C.C.; Stucky, G.D.; Chmelka, B.F. Molecularly ordered inorganic frameworks in layered silicate surfactant mesophases. J. Am. Chem. Soc. 2001, 123, 4519–4529. [Google Scholar] [CrossRef] [PubMed]
  43. Hedin, N.; Graf, R.; Christiansen, S.C.; Gervais, C.; Hayward, R.C.; Eckert, J.; Chmelka, B.F. Structure of a surfactant-templated silicate framework in the absence of 3D crystallinity. J. Am. Chem. Soc. 2004, 126, 9425–9432. [Google Scholar] [CrossRef] [PubMed]
  44. Pines, A.; Gibby, M.G.; Waugh, J.S. Proton-enhanced NMR of dilute spins in solids. J. Chem. Phys. 1973, 59, 569–590. [Google Scholar] [CrossRef]
  45. Wu, X.L.; Zilm, K.W. Complete spectral editing in CPMAS NMR. J. Magn. Reson. A 1993, 102, 205–213. [Google Scholar] [CrossRef]
  46. Palmas, P.; Tekely, P.; Canet, D. Local-field measurements on powder samples from polarization inversion of the rare-spin magnetization. J. Magn. Reson. A 1993, 104, 26–36. [Google Scholar] [CrossRef]
  47. Brouwer, D.H.; Cadars, S.; Eckert, J.; Liu, Z.; Terasaki, O.; Chmelka, B.F. A general protocol for determining the structures of molecularly ordered but noncrystalline silicate frameworks. J. Am. Chem. Soc. 2013, 135, 5641–5655. [Google Scholar] [CrossRef] [PubMed]
  48. Biesinger, M.C.; Lau, L.W.M.; Gerson, A.R.; Smart, R.S.C. Resolving surface chemical states in XPS analysis of first row transition metals, oxides and hydroxides: Sc, Ti, V, Cu and Zn. Appl. Surf. Sci. 2010, 257, 887–898. [Google Scholar] [CrossRef]
  49. Dake, L.S.; Baer, D.R.; Zachara, J.M. Auger parameter measurements of zinc compounds relevant to zinc transport in the environment. Surf. Interface Anal. 1989, 14, 71–75. [Google Scholar] [CrossRef]
  50. Zhao, H.B.; Yu, R.F.; Ma, S.C.; Xu, K.Z.; Chen, Y.; Jiang, K.; Fang, Y.; Zhu, C.X.; Liu, X.C.; Tang, Y.; et al. The role of Cu1–O3 species in single-atom Cu/ZrO2 catalyst for CO2 hydrogenation. Nat. Catal. 2022, 5, 818–831. [Google Scholar] [CrossRef]
  51. Behrens, M.; Studt, F.; Kasatkin, I.; Kühl, S.; Hävecker, M.; Abild-Pedersen, F.; Zander, S.; Girgsdies, F.; Kurr, P.; Kniep, B.-L.; et al. The active site of methanol synthesis over Cu/ZnO/Al2O3 industrial catalysts. Science 2012, 336, 893–897. [Google Scholar] [CrossRef]
  52. Zhang, Z.Q.; Yin, H.R.; Yu, G.D.; He, S.; Kang, J.C.; Liu, Z.M.; Cheng, K.; Zhang, Q.H.; Wang, Y. Selective hydrogenation of CO2 and CO into olefins over sodium and zinc promoted iron carbide catalysts. J. Catal. 2021, 395, 350–361. [Google Scholar] [CrossRef]
  53. Peter, A.; Bernhard, K.; David, D.; Norbert, K.; Thomas, G.; Patrick, L.; Christoph, R.; Kevin, P.; Djuro, B.; Hsin-Yi, W.; et al. The state of zinc in methanol synthesis over a Zn/ZnO/Cu(211) model catalyst. Science 2022, 376, 603–608. [Google Scholar]
  54. Jo, D.Y.; Lee, M.W.; Ham, H.C.; Lee, K.Y. Role of the Zn atomic arrangements in enhancing the activity and stability of the kinked Cu(211) site in CH3OH production by CO2 hydrogenation and dissociation: First-principles microkinetic modeling study. J. Catal. 2019, 373, 336–350. [Google Scholar] [CrossRef]
Figure 1. XRD patterns of ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5.
Figure 1. XRD patterns of ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5.
Nanomaterials 13 03053 g001
Figure 2. TEM, HRTEM, and SAED images of (ac) ZSM-5, (df) Cu@ZSM-5, (gi) Zn@ZSM-5 and (jl) CuZn@ZSM-5 (The red circle represents the HRTEM position).
Figure 2. TEM, HRTEM, and SAED images of (ac) ZSM-5, (df) Cu@ZSM-5, (gi) Zn@ZSM-5 and (jl) CuZn@ZSM-5 (The red circle represents the HRTEM position).
Nanomaterials 13 03053 g002
Figure 3. 27Al MAS NMR spectra of ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5.
Figure 3. 27Al MAS NMR spectra of ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5.
Nanomaterials 13 03053 g003
Figure 4. Single-pulse 29Si MAS NMR spectra of (a) ZSM-5, (b) Cu@ZSM-5, (c) Zn@ZSM-5 and (d) CuZn@ZSM-5 after the removal of the template by calcination. (The dashed line represents the experimental results and the red line represents the fitted accumulated results.)
Figure 4. Single-pulse 29Si MAS NMR spectra of (a) ZSM-5, (b) Cu@ZSM-5, (c) Zn@ZSM-5 and (d) CuZn@ZSM-5 after the removal of the template by calcination. (The dashed line represents the experimental results and the red line represents the fitted accumulated results.)
Nanomaterials 13 03053 g004
Figure 5. 1H-29Si CP/MAS NMR spectra of ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 with a contact time of 8 ms after the removal of the template by calcination.
Figure 5. 1H-29Si CP/MAS NMR spectra of ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5 with a contact time of 8 ms after the removal of the template by calcination.
Nanomaterials 13 03053 g005
Figure 6. Area ratio of the peak at −112 ppm to the total peak area from variable contact-time 1H-29Si CP/MAS NMR spectra for ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5.
Figure 6. Area ratio of the peak at −112 ppm to the total peak area from variable contact-time 1H-29Si CP/MAS NMR spectra for ZSM-5, Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5.
Nanomaterials 13 03053 g006
Figure 7. SXRD experimental patterns (black lines), fitted patterns (red lines) and their difference (blue lines) for (a) Cu@ZSM-5, (b) Zn@ZSM-5 and (c) CuZn@ZSM-5.
Figure 7. SXRD experimental patterns (black lines), fitted patterns (red lines) and their difference (blue lines) for (a) Cu@ZSM-5, (b) Zn@ZSM-5 and (c) CuZn@ZSM-5.
Nanomaterials 13 03053 g007
Figure 8. The relationship between Cu, Zn and MFI framework calculated by SXRD. (a) Cu-1 in [54.6.102] tiling of Cu@ZSM-5, (b) Cu-2 in [62.104] tiling of Cu@ZSM-5, (c) Zn in [54.6.102] tiling of Zn@ZSM-5, (d) Cu in [62.104] tiling of CuZn@ZSM-5, (e) Zn in [54.6.102] tiling of CuZn@ZSM-5. (f) Positions of [54.6.102] (purple) and [62.104] (orange) tilings in the MFI framework.
Figure 8. The relationship between Cu, Zn and MFI framework calculated by SXRD. (a) Cu-1 in [54.6.102] tiling of Cu@ZSM-5, (b) Cu-2 in [62.104] tiling of Cu@ZSM-5, (c) Zn in [54.6.102] tiling of Zn@ZSM-5, (d) Cu in [62.104] tiling of CuZn@ZSM-5, (e) Zn in [54.6.102] tiling of CuZn@ZSM-5. (f) Positions of [54.6.102] (purple) and [62.104] (orange) tilings in the MFI framework.
Nanomaterials 13 03053 g008
Figure 9. High SNR ADF-STEM image of CuZn@ZSM-5. (a) Representative STEM images of CuZn@ZSM-5 along the [010] zone axis, (b) partial enlargement of the three blue marked positions in (a), (c) intensity analysis of the pore center in (b).
Figure 9. High SNR ADF-STEM image of CuZn@ZSM-5. (a) Representative STEM images of CuZn@ZSM-5 along the [010] zone axis, (b) partial enlargement of the three blue marked positions in (a), (c) intensity analysis of the pore center in (b).
Nanomaterials 13 03053 g009
Figure 10. (a) Cu 2p and (b) Zn 2p XPS spectra of Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5. (* Represents satellite peak.)
Figure 10. (a) Cu 2p and (b) Zn 2p XPS spectra of Cu@ZSM-5, Zn@ZSM-5 and CuZn@ZSM-5. (* Represents satellite peak.)
Nanomaterials 13 03053 g010
Figure 11. Performance of CO2 catalytic hydrogenation to methanol over (a) Cu@ZSM-5, (b) Zn@ZSM-5, (c) CuZn@ZSM-5, (d) mixed-particle Cu@ZSM-5 and Zn@ZSM-5 catalysts and (e) dual bed of Cu@ZSM-5 followed by Zn@ZSM-5 catalysts as a function of temperature, and (f) comparison of methanol STY over each catalyst at 533 K. Reaction conditions: 4.0 MPa, H2/CO2/Ar of 72/24/4 and GHSV of 24,000 mL·gcatal−1·h−1.
Figure 11. Performance of CO2 catalytic hydrogenation to methanol over (a) Cu@ZSM-5, (b) Zn@ZSM-5, (c) CuZn@ZSM-5, (d) mixed-particle Cu@ZSM-5 and Zn@ZSM-5 catalysts and (e) dual bed of Cu@ZSM-5 followed by Zn@ZSM-5 catalysts as a function of temperature, and (f) comparison of methanol STY over each catalyst at 533 K. Reaction conditions: 4.0 MPa, H2/CO2/Ar of 72/24/4 and GHSV of 24,000 mL·gcatal−1·h−1.
Nanomaterials 13 03053 g011
Table 1. Metal content: theoretical values and experimental values.
Table 1. Metal content: theoretical values and experimental values.
SampleTheoretical Value aExperimental Value b
Cu (wt.%)Zn (wt.%)Cu (wt.%)Zn (wt.%)
Cu@ZSM-52.07-1.82-
Zn@ZSM-5-1.06-0.91
CuZn@ZSM-52.051.042.230.89
a Calculated by starting synthesis gel. b Calculated by ICP-AES results.
Table 2. Texture results of the samples from N2 adsorption experiments.
Table 2. Texture results of the samples from N2 adsorption experiments.
SampleSBET a
(m2·g−1)
Smicro
(m2·g−1)
Vmicro b
(cm3·g−1)
Vtotal
(cm3·g−1)
Pore Diameter c
(nm)
ZSM-54373370.130.220.52
Cu@ZSM-54102590.100.210.52
Zn@ZSM-54082960.120.200.53
CuZn@ZSM-52851930.070.230.53
a Calculated by the Brunauer–Emmett–Teller (BET) equation. b Calculated by t-plot method. c Calculated from NLDFT adsorption data.
Table 3. The different chemical environments of Si from the 29Si MAS NMR spectra.
Table 3. The different chemical environments of Si from the 29Si MAS NMR spectra.
SampleChemical Environment (%)Si/Al *
(NMR)
Si/Al
(ICP-AES)
Si(OSi)3(OAl)1Si(OSi)4
−101 ppm−105 ppm−112 ppm−116 ppm
ZSM-52.43.283.910.57186
Cu@ZSM-51.63.375.219.98279
Zn@ZSM-51.53.178.117.38782
CuZn@ZSM-51.53.383.611.68375
Si / Al   = n = 0 4 I Si nAl / n = 0 4 0.25 n [ I Si ( nAl ) ] .
Table 4. The different chemical environments of Cu obtained from the XPS spectra.
Table 4. The different chemical environments of Cu obtained from the XPS spectra.
SampleChemical Environment (%)Area Ratio of Cu-2:Cu-1
Cu 2p1/2Cu 2p3/2
Cu-1
(956.0 eV)
Cu-2
(953.7 eV)
Cu-1
(935.3 eV)
Cu-2
(933.7 eV)
Cu@ZSM-512.5%15.5%32.0%40.0%1.25
CuZn@ZSM-5-34.1%-65.9%-
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Ding, H.; Zhang, J.; Feng, W.; Yao, Q.; Zhang, L.; Ren, Y.; Ye, L.; Yue, B.; He, H. Precise Confinement and Position Distribution of Atomic Cu and Zn in ZSM-5 for CO2 Hydrogenation to Methanol. Nanomaterials 2023, 13, 3053. https://0-doi-org.brum.beds.ac.uk/10.3390/nano13233053

AMA Style

Ding H, Zhang J, Feng W, Yao Q, Zhang L, Ren Y, Ye L, Yue B, He H. Precise Confinement and Position Distribution of Atomic Cu and Zn in ZSM-5 for CO2 Hydrogenation to Methanol. Nanomaterials. 2023; 13(23):3053. https://0-doi-org.brum.beds.ac.uk/10.3390/nano13233053

Chicago/Turabian Style

Ding, Hongxin, Jinwen Zhang, Wenhua Feng, Qingying Yao, Li Zhang, Yuanhang Ren, Lin Ye, Bin Yue, and Heyong He. 2023. "Precise Confinement and Position Distribution of Atomic Cu and Zn in ZSM-5 for CO2 Hydrogenation to Methanol" Nanomaterials 13, no. 23: 3053. https://0-doi-org.brum.beds.ac.uk/10.3390/nano13233053

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop