Next Article in Journal
Relationship between Immune Cells, Depression, Stress, and Psoriasis: Could the Use of Natural Products Be Helpful?
Next Article in Special Issue
Decontamination Efficiency of Thermal, Photothermal, Microwave, and Steam Treatments for Biocontaminated Household Textiles
Previous Article in Journal
Enhanced Anti-Skin-Aging Activity of Yeast Extract-Treated Resveratrol Rice DJ526
Previous Article in Special Issue
Antibacterial Properties of Non-Modified Wool, Determined and Discussed in Relation to ISO 20645:2004 Standard
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Silver Nanowires and Silanes in Hybrid Functionalization of Aramid Fabrics

by
Alicja Nejman
1,2,
Anna Baranowska-Korczyc
1,
Katarzyna Ranoszek-Soliwoda
2,
Izabela Jasińska
1,
Grzegorz Celichowski
2 and
Małgorzata Cieślak
1,*
1
Łukasiewicz Research Network–Textile Research Institute, Brzezinska St. 5/15, 92-103 Lodz, Poland
2
Department of Materials Technology and Chemistry, Faculty of Chemistry, University of Lodz, Pomorska St. 163, 90-236 Lodz, Poland
*
Author to whom correspondence should be addressed.
Submission received: 22 February 2022 / Revised: 11 March 2022 / Accepted: 14 March 2022 / Published: 17 March 2022
(This article belongs to the Special Issue Advances in Textile Materials Chemistry)

Abstract

:
New functionalization methods of meta- and para-aramid fabrics with silver nanowires (AgNWs) and two silanes (3-aminopropyltriethoxysilane (APTES)) and diethoxydimethylsilane (DEDMS) were developed: a one-step method (mixture) with AgNWs dispersed in the silane mixture and a two-step method (layer-by-layer) in which the silanes mixture was applied to the previously deposited AgNWs layer. The fabrics were pre-treated in a low-pressure air radio frequency (RF) plasma and subsequently coated with polydopamine. The modified fabrics acquired hydrophobic properties (contact angle ΘW of 112–125°). The surface free energy for both modified fabrics was approximately 29 mJ/m2, while for reference, meta- and para-aramid fabrics have a free energy of 53 mJ/m2 and 40 mJ/m2, respectively. The electrical surface resistance (Rs) was on the order of 102 Ω and 104 Ω for the two-step and one-step method, respectively. The electrical volume resistance (Rv) for both modified fabrics was on the order of 102 Ω. After UV irradiation, the Rs did not change for the two-step method, and for the one-step method, it increased to the order of 1010 Ω. The specific strength values were higher by 71% and 63% for the meta-aramid fabric and by 102% and 110% for the para-aramid fabric for the two-step and one-step method, respectively, compared to the unmodified fabrics after UV radiation.

Graphical Abstract

1. Introduction

Due to their low density, high tensile strength, excellent thermal stability, high specific strength, and modulus of elasticity, aramid fibers are widely used in special clothes accessories and technical products [1]. Their weakness, however, is their poor resistance to UV radiation. Aramids absorb UV radiation in the range of 300 to 400 nm, which results in breaking of the intermolecular bonds in the polymer that causes deterioration of the mechanical properties [2,3]. Therefore, it is important to protect them against UV radiation such as by modification with nanosilver, which also provides antibacterial and antistatic properties. Such functionalization significantly extends the scope of their application, such as materials for thermal sensors in smart clothes, for the protection of electronic communication, and in aviation [4,5,6]. The molecular structure of aramid fibers, which consist of aromatic rings and amide groups, makes them highly crystalline [7,8]. Due to the smooth and chemically inert surface, they show poor adhesion to modifiers. In order to improve the functionalization efficiency, an initial surface modification is performed through plasma activation and deposition of a polydopamine thin film by oxidative polymerization of dopamine [9]. The activation increases the free surface energy of aramid fibers and creates more reactive sites, enabling better binding between the polydopamine and the aramid surface [9,10,11]. Polydopamine is a biopolymer that forms a coating on the fiber surface through induced dopamine oxidative self-polymerization. This process enables the creation of carboxyl, amine, and catechol functional groups in order to strengthen the bond between the fiber and the modifier and improve the physical properties of the composites [12,13,14]. Polydopamine shows adhesion for most types of inorganic and organic surfaces, including precious metals, oxides, polymers, semiconductors, and ceramics [13,15]. Studies on the adhesion mechanism of the polydopamine film show that functional groups create covalent and non-covalent connections with inorganic or organic materials [15,16,17,18]. This type of preliminary modification increases the deposition efficiency of silver nanoparticles and improves the durability of the coating [9,19,20,21]. Silver nanowires (AgNWs) are one type of nanomodifier used for the multifunctionalization of textile materials. They have two UV absorption peaks; the peak at 350 nm can be attributed to surface plasmon resonance (SPR) along the silver nanowires, and the peak at about 380 nm can be considered the transverse direction of the SPR [22,23]. AgNWs absorb UV radiation, constituting a protective barrier for the fibrous structure covered with them, but they can also degrade. Air humidity has a significant influence on the degradation under the influence of UV radiation [24]. For higher air humidity, the oxygen and water contained in the air under the influence of UV radiation can create ozone and hydroxyl groups, which can initiate oxidation, hydrolysis, and photodegradation processes of the AgNWs [24,25]. For protection against UV radiation, silanes are used [26,27,28,29] because they have the ability to reflect UV radiation [28]. Hydrophobic silane-based textile materials are usually produced by surface treatment with mixtures of silane agents and silane cross-linkers [28,30]. One of the silanes used for the modification is 3-aminopropyltriethoxysilane (APTES), which contains a polar and chemically active aminopropyl group and three easily hydrolysable alkoxy groups. The hybrid organo-silica film obtained by APTES hydrolysis is hydrophilic, and the water contact angle measured by Zeng et al. [31] for the APTES film was 50°. The addition of diethoxydimethylsilane (DEDMS) to tetraethoxysilane (TEOS) before the hydrolysis increased the hydrophobicity of the obtained coatings was studied by Zhang et al. [32]. Souza et al. [33], for a mixture of APTES with (3-glycidoxypropyl) trimethoxysilane (GPTMS) (ratio of 2:1), obtained a coating with a water contact angle of 109.7°. Hasanzadeh et al. [34] coated a polyester-viscose fabric with silica nanoparticles prepared from TEOS to obtain a rough and hydrophobic surface. The fabric was then treated with functionalized polydimethylsiloxane (PDMS) to reduce the surface free energy. This fabric became hydrophobic with a contact angle of 151°. APTES is most often used as a stabilizer and a fastener to immobilize silver nanoparticles on the fiber surface [35].
In this work, meta- and para-aramid fabrics were modified with AgNWs and a mixture of silanes, APTES, and DEDMS. There were two methods of modification tested, a one-step method using a mixture of silanes with a AgNWs colloid (ratio of 1:10) and a two-step method (layer-by-layer), in which a mixture of silanes was applied on the AgNWs coating. The aim of the research was to protect aramid fabrics against UV radiation, improve the durability, conductivity, and hydrophobic properties, and assess which modification method is more effective.
Obtained results will have a significant impact on the development of knowledge in the field of material engineering, surface physico-chemistry, and functionalization of aramid materials. The functionalization of aramid textile materials with AgNWs and silanes is an original strategy of improving functionality of aramid fabrics, by giving them mechanical resistance to UV radiation, hydrophobicity, and conductivity. Protection against UV radiation extends the usage of modified aramid fabrics, which has a beneficial effect on the environment. In addition, hydrophobicity reduces the contamination, including biofouling, and protects AgNWs against corrosion. In turn, imparting conductive properties aims to create conductive paths between elements and to protect electronic components against electrostatic discharge (ESD) in textronic products. Thanks to the combination of the functional properties of the AgNWs, silanes, and aramids, we developed modified aramid fabrics, which can be used in many fields, e.g., in the automotive and military industry, in protective clothing in high-risk occupations, to monitor vital functions or the level of available oxygen, and also in everyday life as textile materials for tents, umbrellas, and covering fabrics, etc.

2. Materials and Methods

2.1. Materials

Meta-aramid (poly (isophthalates-1,3-fenylodiamid)) (mAr) fabric with a plain-weave and mass per unit area of 205 g/m2 made of 25 × 2 tex yarn (number of threads: in warp—230/10 cm, in weft—160/10 cm), (Newstar®, Yantai Tayho Advanced Materials Co., Ltd., Yantai, China) and para-aramid (poly (1,4-terephthalate-fenylodiamid)) (pAr) fabric with a plain-weave and mass per unit area of 165 g/m2 made of 20 × 2 tex yarn (number of threads: in warp—240/10 cm, in weft—150/10 cm), (Kevlar®, DuPont, Londonderry, UK) were studied. Both fabrics were made in Łukasiewicz Research Network-Textile Research Institute using the harness loom (CCI Tech. Inc., New Taipei City, Taiwan).

2.2. Methods

2.2.1. Functionalization Methods

Preparation of Silver Nanowires (AgNWs) Colloid

The synthesis of AgNWs was described in a previous work [36]. In brief, AgNWs were synthesized by reduction of silver nitrate (AgNO3, 99.9%, Sigma Aldrich, Gillingham, UK) with ethylene glycol (C2H6O2, Avantor, Gliwice, Poland) in the presence of polyvinylpyrrolidone (PVP, 55,000 g/mol, Sigma Aldrich, UK).
The synthesis was performed in a Radleys 1l Reactor-Ready (Radleys, Essex, United Kingdom) reactor equipped with a mechanical stirrer, working at a speed of 150 RPM. The reactor has a double heating jacket, allowing for precise temperature control performed by an external thermostat during the entire synthesis. The temperature was set at 170 ± 2 °C.
A total of 600 mL of ethylene glycol, 30 g of PVP, and 0.42 g of sodium chloride (NaCl, CHEMPUR, Piekary Śląskie, Poland) were heated to 167 °C (constant temperature control) and stirred at 150 RPM to obtain a homogenous solution. Then, a mixture of 6.12 g of AgNO3 in 300 mL of ethylene glycol was added with a peristaltic pump at a rate of 3.33 mL/min for 90 min into the heated solution of ethylene glycol, PVP, and NaCl. When the silver precursor solution was added, the colloid was stirred at 150 RPM and heated for 60 min at 167 °C.
After the synthesis, the solution was air-cooled to about 25 °C. To remove ethylene glycol and excess PVP from the colloid, the subsequent, small parts of the solution were diluted with acetone (C3H6O, 99,5%, Avantor, Gliwice, Poland) with a ratio of 1:10 and shaken for 10 min. Then, the silver nanowires were dispersed in anhydrous ethyl alcohol (C2H6O, 99,8%, Avantor, Gliwice, Poland). The obtained AgNWs colloid concentration was 4000 ppm, the length of the AgNWs was about 10 ± 2 µm, and the diameter was about 42 ± 3 nm.

Low-Pressure Air RF Plasma Treatment of Aramid Fabrics

Para-aramid and meta-aramid fabrics were washed in diethyl ether for 30 min and dried at 25 °C. Next, both fabrics were treated with a low-pressure air RF plasma (Zepto plasma system, Model 2. Diener Electronic, Ebhausen, Germany) for 10 min. The pressure in the plasma chamber was set at 0.3 mbar with laboratory air (Linde Gaz, Kraków, Poland) with the purity: 20% of O2 and 80% of N2 (40% relative humidity) as the working gas. The power of the plasma was set at 50 W and the generator frequencies was 40 kHz.

Polydopamine Functionalization of Aramid Fabrics

A dopamine solution with a concentration of 2 g/L was prepared by dissolving dopamine hydrochloride (Sigma Aldrich, UK) in distilled water. The pH of the solution was adjusted to 8.3 by adding tris/glicyne buffer (BIO RAD, Warszawa, Poland). The plasma treated aramid fabrics were immersed in the dopamine solution for 24 h (Figure 1a). Under the same conditions, a polydopamine coating was prepared on the surface of the aluminum plate. This material was used for the acquisition of a reference FTIR spectrum of pure polydopamine. After that, all samples were rinsed with distilled water three times and then dried for 24 h at 25 °C.

Silanes Sol Preparation

APTES (Unisil, Tarnów, Poland) and DEDMS (Sigma Aldrich, Gillingham, United Kingdom) differ in their chemical structure, brittleness, and hydrophobicity. To prepare the AgNWs and silane modified aramid fabrics, silanes sol was prepared by mixing 15.00 g of APTES, 1.12 g of DEDMS, and 3.93 g of 1 M HCl (Avantor, Gliwice, Poland). The silanes mixture was shaken for 30 min. Next, ethyl alcohol (C2H6O, 99.8%, Avantor, Gliwice, Poland) was added at 50% by volume of the silanes mixture.

AgNWs and Silanes Functionalization of Aramid Fabrics

The one-step (mixture) and two-step (layer-by-layer) methods were used for the functionalization of aramid fabrics with AgNWs and silanes (Figure 1b). In the one-step method, aramid fabrics were 5-fold dipped in a mixture of a AgNWs colloid (Ag) with 10 wt.% silanes sol (S) for 1 min. After the mixture was applied every time, the fabrics were dried in an oven at 100 °C for 1 h. The fabrics modified with the mixture (Ag + S) are denoted as mAr/RF/PD/5Ag+S and pAr/RF/PD/5Ag+S for the meta- and para-aramid fabric, respectively.
In the two-step method, fabrics were dipped in the AgNWs colloid for 1 min and dried at 25 °C. The AgNWs colloid (Ag) was applied 5 times. Then, the fabrics were dipped 1 time in the silanes sol (S) and then dried in an oven at 100 °C for 1 h. The fabrics modified with the layer-by-layer (Ag/S) method are denoted as mAr/RF/PD/5Ag/S and pAr/RF/PD/5Ag/S for the meta- and para-aramid fabric, respectively.
Moreover, as control samples, aramid fabrics were modified with AgNWs. A 1-fold (mAr/RF/PD/1Ag and pAr/RF/PD/1Ag) and 5-fold (mAr/RF/PD/5Ag and pAr/RF/PD/5Ag) colloid application was used.
In Table 1, the values of mass per unit area of the reference and functionalized aramid fabrics are summarized.

UV Irradiation

The UV irradiated unmodified and modified fabrics were placed between two (100 W) LED diodes with the maximum wavelength of the emitted light at 365 nm for 96 h. The irradiance (W) was determined by using the CUV 4 irradiance sensor (Kipp & Zonen B.V., Delft, Netherlands) to measure the intensity of the light in the UV range (305–385 nm). The supplied irradiation energy (P) was calculated from Equation (1) [37] and determined to be 46,719 kJ/m2 for one LED diode.
P = t · 3.6 · Σ W n
where P is the irradiation energy (kJ/m2), t is the irradiation time (h), W is the irradiance (W/m2), and n is the number of measurements during the irradiation time t.

2.2.2. Characterization Methods

SEM/EDS Analysis

The morphology and chemical composition analysis were performed using a scanning electron microscope (SEM) (Nova NanoSEM 450 FEI, Hillsboro, OR, USA) and VEGA 3 (TESCAN, Brno, Czech Republic) with an energy dispersive spectroscopy (EDS) X-ray microanalyzer INCA Energy (Oxford Instruments Analytical, High Wycombe, United Kingdom) with a magnification of 2500×, 10,000×, and 20,000×. A total of three EDS spectra were recorded for each sample, and mean values of the weight percentage of the elements were determined.

Optical Microscopy

The images of the fabric surface before and after the abrasion process were acquired using an optical microscope DSX1000 (OLYMPUS, Tokyo, Japan) and using the DEPH function to increase the depth of field. A magnification of 300× was used for all images.

FTIR Analysis

FTIR/ATR (Fourier transform infrared spectroscopy/attenuated total reflectance) spectra of reference and plasma-treated yarns were recorded in the range 600–4000 cm−1 using Nicolet IS 50 spectrometer (Thermo Fisher Scientific Inc., Bartlesville, OK, USA) with GATR (grazing angle attenuated total reflectance) accessory (Harrick Scientific Products Inc., New York, NY, USA) using the MCT (mercury-cadmium-telluride) detector. This accessory allows to collecting spectra from the surface of the fibers at a depth of about up to 50 nm.

Surface Properties

The analysis of the surface properties of the fabrics was performed by the goniometric method using the goniometer PGX (Fibro System AB, Stockholm, Sweden). In order to determine the surface free energy (γs), three standard liquids with known surface tensions and different values of dispersive and polar components were applied (Table 2). The drop of liquid with a volume of 4 µL was applied. A total of three repetitions for each sample were used. The surface free energy was determined according to the Wu model (Equation (2)), which is based on the assumptions of the Owens-Wendt model [7,38,39,40,41,42] but describes the intermolecular interaction using the harmonic mean.
γl(1+cosθ) = 4((γldγsd)/γld + γsd + γlpγsplp + γsp) and γs = γsd + γsp
where γsd and γsp are the dispersive and polar components of a solid, respectively, and γld and γlp are the dispersive and polar components of a liquid, respectively.

Specific Strength

The study of the specific strength of the fabrics before and after UV irradiation was performed by using the Instron 3367 Test Machine (United Kingdom) in accordance with PN-EN ISO 13934-1:2013-07 Textiles—Tensile properties of flat products—Part 1: Determination of maximum force and relative elongation at maximum force by the strip method. A total of five repetitions for each sample were used. Samples were conditioned for 24 h at a temperature of 21.0 ± 1.0 °C and a relative humidity (RH) of 64.4 ± 0.1% and then tested in the same conditions.

Abrasion Resistance

The resistance to abrasion of the fabrics before and after UV irradiation was studied using the Martindale unit (United Kingdom) in accordance with PN-EN ISO 12947-2:2017-02 Textiles—Determination of the abrasion resistance of fabrics by Martindale method—Part 2: Determination of specimen breakdown. A total of three repetitions for each sample were used. Samples were conditioned for 24 h at a temperature of 21.1 ± 0.1 °C and an RH of 64.4 ± 0.1% and were tested in the same conditions. A standard woolen fabric was used as an abrasive cloth. An abrasive load of 12 kPa was applied.

Conductivity

The electrical surface resistance (Rs) and electrical volume resistance (Rv) of the fabrics before and after UV irradiation were determined according to the PN-EN 1149-1:2008 for Rs and PN-EN 1149-2:1999+A1:2001 for Rv, using a set of standard electrodes and a 6206 teraohmmeter (ELTEX, Weil am Rhein, Germany). The fabrics were conditioned for 24 h in the HCZ 0030 L(M) chamber (Heraeus, Hanau, Germany) at a temperature of 23.0 ± 2.0 °C and an RH of 25.0 ± 5.0% and were tested in the same conditions.

3. Results and Discussion

3.1. Modification of the Aramid Fabrics with Low-Pressure Air RF Plasma and Polydopamine

The surface of the meta- (Figure 2a) and para-aramid (Figure 2a) fibers is smooth with visible longitudinal cracks. Aramid fibers have a fibrillar structure. Activation in low-pressure RF plasma causes an increase in the unevenness and surface roughness (Figure 1b and Figure 2b).
The dopamine solution prepared for the functionalization of the plasma-activated aramid fabrics was colorless and transparent. During the oxidative autopolymerization of dopamine, the color of the solution quickly turned pink as catechol was oxidized to benzoquinone. Then, the pink solution slowly turned to dark brown. This indicates that after polymerization, the reaction of melanin formation takes place, resulting in the creation of polydopamine (PD) with a high strength of irreversible covalent bonds on the matrix. After modification, polydopamine formed a layer on the surface of both types of fibers (Figure 2c and Figure 3c).
The presence of the polydopamine coating on the aramid fiber surface was observed during the SEM analysis and confirmed by the FTIR spectroscopy results (Figure 4). In Table 3, the characteristic bands and their wavenumbers for the pAr fabric and polydopamine are presented. After application of the dopamine coating on the pAr fabric, an increase in the band intensity at 698 cm−1, corresponding to the C–H bond out-of-plane of the substituted aromatic ring, and at 1513 cm−1, corresponding to the C=N bond stretching vibrations of the aromatic ring, in relation to the unmodified pAr (Figure 3a) is observed. In the spectrum for the pAr/RF/PD fabric, bands are present in the spectrum for polydopamine but not in the spectrum for the reference pAr fabric. These are the bands at 911 cm−1 characteristic of the bending vibrations of the CONH bond and CN stretching, at 1440 cm−1 corresponding to the stretching vibrations of the C=C bond of the aromatic ring (Figure 4a), and at 3175 cm−1 corresponding to the stretching vibrations of the N–H bond (Figure 4b).

3.2. AgNWs and Silanes Modified Aramid Fabrics before and after UV Irradiation

SEM analysis shows that the surface of both aramid fibers after the 1-fold application of AgNWs (mAr/RF/PD/1Ag and pAr/RF/PD/1Ag) is covered unevenly (Figure 5a and Figure 6a). After the 5-fold application, the coating is uniform (Figure 4b), with few areas without AgNWs (Figure 6b). AgNWs are found both on the surface of the fibers and inside the fabric structure. After application of the Ag+S mixture (Figure 5c and Figure 6c), the AgNWs were embedded inside the silanes coating and deposited both on the surface of the fibers and in the spaces between them. In the case of the layer-by-layer method (Figure 5d and Figure 6d), a layer of silanes covers the surface of the fabric with AgNWs. There are also fibers with AgNWs that protrude above the silanes surface.
EDX analysis of the mAr and pAr fabric shows the presence of C, N, and O (Table 4). For the mAr fabric, the content of C, N, and O is 68, 11, and 20 wt.%, respectively. For the mAr/RF/PD/1Ag fabric, the content of Ag is 3 wt.%, and for mAr/RF/PD/5Ag, it is 6-fold higher (Table 4). With the increase in the multiplicity of the AgNWs application, the content of C, N, and O decreased, which proves the effective coverage of the aramid fibers with AgNWs. For mAr/RF/PD/5Ag+S, the C and N content does not change significantly, and the O content, which is derived from the ethoxyl groups in silanes, increases by about 50% compared to mAr/RF/PD/5Ag. A decrease in the C content by 26% and an increase in the O and N content by 70% and 24%, respectively, are noted for mAr/RF/PD/5Ag/S in relation to mAr/RF/PD/5Ag. These changes are due to the presence of the silanes layer, which contains ethoxy groups and an amino group. The Ag content on the fiber surface is about 60% and 30% lower for mAr/RF/PD/5Ag+S and mAr/RF/PD/5Ag/S compared with mAr/RF/PD/5Ag. The Si content is 5 wt.% and 7 wt.% for mAr/RF/PD/5Ag+S and mAr/RF/PD/5Ag/S, respectively.
The content of C, N, and O for the pAr fabric is 66, 13, and 19 wt.%, respectively. In the case of pAr/RF/PD/1Ag, the Ag content is 6 wt.%, and after the 5-fold application, it is 3.5 times higher. The content of C, N, and O decreases with the increase in the number of AgNWs applications, which indicates the effective coverage of the fibers with AgNWs. For pAr/RF/PD/5Ag+S, the C and N content stays at the same level in relation to pAr/RF/PD/5Ag. The O content increases by 48%, which is due to the presence of ethoxyl groups in the silanes. For pAr/RF/PD/5Ag/S, the C content is lower by 22%, and the N and O content is higher by 46% and 72%, respectively, which, similarly to the meta-aramid fabric, is due to the surface being covered with silanes. For pAr/RF/PD/5Ag+S and pAr/RF/PD/5Ag/S, the Ag content on the fiber surface is lower by about 64% and 42%, respectively, than for pAr/RF/PD/5Ag. The Si content is 5 wt.% for pA/RF/PD/5Ag+S and 6 wt.% for pAr/RF/PD/5Ag/S.
After 96 h of UV irradiation of the unmodified mAr (Figure 7a) and pAr (Figure 8a) fabrics, the roughness of the fibers surface increased, and polymer fragments were present on the surface. The UV irradiation caused degradation of the AgNWs on the fabrics, as evidenced by silver precipitates on their surface (Figure 7b insert, Figure 8b insert). The coating on the mAr and pAr fibers modified with the Ag + S mixture was cracked (Figure 7c and Figure 8c), and coating defects were visible, which proves that fragments of the Ag + S coating were detached (Figure 7c). UV radiation causes breaking of the polysiloxane bonds and photo-oxidation, which induces the formation of silanol and carbonyl groups [27]. In the case of the layer-by-layer method, the AgNWs did not degrade and did not change their morphology (Figure 7d and Figure 8d). In the mixture method, the AgNWs were more exposed to the UV radiation due to the thin coating of silanes compared with the layer-by-layer method. This may cause the degradation of AgNWs and damages in silanes coating.

3.3. Surface Properties

Table 5 presents the values of contact angles for water (ΘW), formamide (ΘF), and diiodomethane (ΘDIM) for the unmodified and modified fabrics.
For the mAr fabric, the ΘW value is 64°, and after plasma activation, it decreases by 70%. For the pAr fabric, the ΘW value is 20% higher than for the mAr fabric. Plasma treatment reduced the ΘW value by 84%. The decrease in the ΘW value of pAr/RF is greater than for mAr/RF because of the chemical structure of both aramids and the higher degree of crystallinity of para-aramid, whose structure is more rigid and orderly, which causes greater changes on the fibers surface as a result of plasma etching [7]. After the application of the polydopamine coating, for the mAr/RF/PD and pAr/RF/PD fabrics, the value of ΘW is 0°. The decrease in the ΘW value is due to the presence of active polar functional groups on the surface, such as –OH, –NH2, or –NH (Figure 4), which interact with the polar liquid. A decrease in the ΘW value was also observed by Sabdin et al. [42], who modified polypropylene (PP) meshes by immersing them in 10 mM dopamine buffered with TRIS at pH 8.5 for 24 h. Then, the PP meshes were washed several times with distilled water and dried at 40 °C. The ΘW value decreased from 138.9° to 74.1°. Jiang et al. [43] immersed a PP membrane for 24 h in a 1.0 g/L aqueous dopamine solution prepared by dissolving 0.25 g of dopamine in 250 mL of deionized water. Then, 1 mL of 1 M NaOH was added to the solution to adjust the pH to 9. The ΘW value decreased from 117.5° to 54.3°. Chen et al. [44] observed a decrease in the ΘW value from 143.7° to 134.2° after modification of the PP nonwoven fabric in an aqueous solution of dopamine hydrochloride at a concentration of 2 g/L and buffered with TRIS (pH = 8.5) for 24 h at 60 °C and then the samples were washed four times with ultrasounds and dried in a vacuum at 60 °C. This indicates the exposure of hydroxyl and amine groups in polydopamine on the nonwoven surface, which causes the increase in the wettability.
The ΘW values for both aramid fabrics with AgNWs are comparable and higher than for the unmodified fabrics, and their hydrophobicity increases with the increasing number of AgNWs deposited.
Fabrics modified with the mixture and layer-by-layer methods are hydrophobic. The mAr/RF/PD/5Ag+S and pAr/RF/PD/5Ag+S fabrics have the highest ΘW values, which are 125° and 120°, respectively. For the mAr/RF/PD/5Ag/S and pAr/RF/PD/5Ag/S fabrics, the ΘW values are 112° and 114°, respectively. Zeng et al. [31] reported that the water contact angle of the APTES film is 52°, which means that APTES is hydrophilic. In turn, Zhang et al. [32] measured the contact angle of a DEDMS/TEOS silica aerogel (ratio of 0.26), which was 139.9°, while TEOS is hydrophilic [45].
The value of the surface free energy (γs) for the mAr fabric is 39.8 mJ/m2, which is lower than for the pAr fabric by about 35% (Figure 9a,b). Plasma treatment and modification with polydopamine resulted in a significant increase in the γs values by about 68% and 84%, respectively, for mAr and by about 87% and 83% for pAr fabrics in relation to the unmodified fabrics. After the 1- and 5-fold AgNWs application, the γs value slightly decreased with the increase in the modification multiplicity for both types of aramid fabrics and is slightly lower in relation to the unmodified fabrics. The γs values for the aramid fabrics modified with silanes by both methods are a little lower than for the fabrics after the 5-fold AgNWs application.
The dispersion component value (γsd) of the mAr fabric is 23.8 mJ/m2, which is lower than that of the pAr fabric by about 50%. The plasma treatment causes a 52% increase and 21% decrease in the γsd component for the mAr/RF and pAr/RF fabric, respectively. The decrease in γsd for the pAr fabric after plasma treatment in comparison with the mAr fabric is related to the higher degree of crystallinity and the fibrillization phenomenon of the reference pAr fabric (Figure 3a). For mAr fabric surface, the enlargement of the surface roughness is observed after plasma treatment (Figure 2b), which causes the increase in the γsd value. After modification with polydopamine, the value of the γsd component decreases in relation to the unmodified fabrics as result of the formation of a layer of polydopamine on the surface of the fibers (Figure 2c and Figure 3c). For both fabrics, after the 1-fold AgNWs application, the γsd values are comparable. The lower γsd value for pAr/RF/PD/1Ag compared with the reference fabric is caused by the fibrillization process, which significantly affects the dispersion component value. For the 5-fold AgNWs modified fabrics, the γsd values are still comparable and lower than for the 1-fold AgNWs modification, which may be related to the smoothing of the discontinuous surface after successive AgNWs applications. For both aramid fabrics modified with silanes by the mixture and layer-by-layer method, the γsd values are lower in relation to the fabrics after the 5-fold AgNWs application. Slightly higher γsd values are found for the layer-by-layer method, which may be because of the visible AgNWs coated fibers that protrude above the smooth silane surface.
The value of γsp for mAr is 16.0 mJ/m2, which is six times higher than the value for pAr. After plasma treatment, the γsp values increase and are comparable for both fabrics. The polydopamine application causes a further increase in the γsp values by a factor of 2 and 1.7 for mAr/RF/PD and pAr/RF/PD, respectively. For fabrics modified with silanes by both methods, the γsp values are lower compared to the unmodified fabrics. The values of the polar components are higher than the dispersive component values only for the fabrics modified with polydopamine. Unmodified fabrics have a smooth surface with numerous longitudinal cracks and fibrils. The surface is chemically inert, and there are no active functional groups. After application of polydopamine, an increase in γsp in relation to γsd is caused by an increase in the polarity of the polydopamine surface due to the presence of active functional groups on the fiber surface: –OH, –NH2, or –NH (Figure 4).

3.4. The Durability before and after UV Irradiation

3.4.1. Specific Strength

The specific strength of the mAr fabric (8.6 N/tex) (Figure 10a) is 4.5 times lower than that of the pAr fabric, which does not change for mAr/RF/PD/5Ag and mAr/RF/PD/5Ag/S. For mAr/RF/PD/5Ag+S, the specific strength is higher than for the mAr fabric by about 12%. In the case of the modified pAr fabrics, a decrease by about 19%, 14%, and 17% is observed for pAr/RF/PD/5Ag, pAr/RF/PD/5Ag+S, and pAr/RF/PD/5Ag/S, respectively, compared to the unmodified fabric. The higher specific strength values after the application of the Ag+S mixture compared with the AgNWs modified fabrics are probably due to the stronger cross-linking of AgNWs with silanes, which occurred both on the surface of the fabric fibers and in the spaces between the fibers. For the layer-by-layer method, the cross-linking between the AgNWs and the silanes layer takes place only on the surface. The layer-by-layer modification does not change the specific strength of the fabrics in relation to the fabrics with AgNWs.
After 96 h of UV irradiation, an almost 50% decrease in the specific strength is observed for the mAr fabric (Figure 10a). The specific strength is higher by 40%, 71%, and 63% for mAr/RF/PD/5Ag, mAr/RF/PD/5Ag+S, and mAr/RF/PD/5Ag/S, respectively, compared with the mAr fabric after UV irradiation. For the unmodified pAr fabric, there is a 60% decrease in the specific strength. For pAr/RF/PD/5Ag, pAr/RF/PD/5Ag+S, and pAr/RF/PD/5Ag/S (Figure 10b), their specific strength values are 58%, 102%, and 111% higher than for the UV irradiated pAr fabric, respectively. The significantly higher specific strength values after the AgNWs and silanes mixture and layer-by-layer modification is related to the reflection of UV radiation by silanes, which protects the AgNWs and aramid from UV degradation. Shi et al. [28] also observed the effect of the silane layer on the reflectance of UV radiation for a cotton fabric modified with graphene oxide and a KH570 silane layer. Tragoonwichian et al. [29] modified a cotton fabric using vinyletriethoxysilane, which significantly reduced the transmittance of UV radiation through the fabric.

3.4.2. Abrasion Resistance

The mAr fabric is abrasion resistant. After 100,000 cycles (Figure 11a), no breakage of the threads is observed (Figure S1a, Supplementary Materials). For the pAr fabric, thread abrasion (Figure S1b, Supplementary Materials) occurs after 5000 cycles (Figure 11b), probably due to the less ordered structure and lower degree of crystallinity of mAr than of pAr. For the mAr/RF/PD/5Ag and mAr/RF/PD/5Ag+S fabric, a decrease in the number of abrasion cycles by 40,000 compared to the mAr fabric is observed, which proves that AgNWs reduce the abrasion resistance of meta-aramid. In the case of the para-aramid fabrics, the application of AgNWs and a mixture of AgNWs and silanes improves the abrasion resistance and increases the number of abrasion cycles (Figure 11b) by 7000 and 75,000, respectively. For the layer-by-layer method, no thread damage is observed for both fabrics after 100,000 abrasion cycles.
After UV exposure, the abrasion resistance of the mAr fabric decreased, the breakage of the threads is observed (Figure S1a, Supplementary Materials), and the number of abrasion cycles decreases by a factor of seven. For the mAr/RF/PD/5Ag and mAr/RF/PD/5Ag+S fabric, the number of abrasion cycles is three times higher than that of the mAr fabric after UV irradiation. For the pAr fabric, the number of abrasion cycles does not change after UV exposure. For the modified fabrics, it is almost four times and 18 times higher for pAr/RF/PD/5Ag and pAr/RF/PD/5Ag+S, respectively, compared to the UV irradiated pAr fabrics. For the layer-by-layer method, after UV irradiation, no breakage of the fibers is observed after 100,000 cycles for both types of aramids, as before UV exposure (Figure S1b, Supplementary Materials).

3.5. Conductive Properties

The unmodified mAr and pAr fabrics are non-conductive, and their electrical surface resistance (Rs) is 1.30 × 1012 Ω and 1.26 × 1012 Ω (Figure 12a), respectively. For both aramid fabrics after the 5-fold AgNWs application, a significant decrease in Rs values by 10 orders of magnitude is observed. For both aramid fabrics modified with silanes by the mixture and the layer-by-layer method, a decrease in the Rs value by eight and nine orders of magnitude, respectively, is observed compared with the reference fabrics.
The electrical volume resistance (Rv) value is 1.30 × 1012 Ω and 1.06 × 1012 Ω (Figure 12b) for the mAr and pAr fabrics, respectively. After the 5-fold AgNW application, the Rv value decreases by 10 orders of magnitude for both fabrics. After the AgNWs and silanes mixture and layer-by-layer modification, the Rv values are lower than those of the unmodified fabrics by nine orders of magnitude.
The slightly higher values of Rs and Rv for the fabrics modified with silanes by the mixture and layer-by-layer method compared to the fabrics with only AgNWs are due to the presence of silanes, which, on aramid fabrics, have higher Rs and Rv values of 5.98 × 107 Ω and 3.77 × 107 Ω, respectively, for the mAr fabric and 3.30 × 108 Ω and 6.91 × 107 Ω, respectively, for the pAr fabric. Silanes can be a barrier to the flow of electrons through AgNWs. Moreover, higher values of both resistances are found for the mixture method than for the layer-by-layer method, which may be due to the AgNWs being covered by silanes, which limits their direct connection with each other (which can be seen in the SEM images, Figure 7c and Figure 8c). On the other hand, for the layer-by-layer method, fibers that protrude above the silanes layer are densely covered with AgNWs, which create conductive paths. Under the silanes layer, both on the surface and between the fibers, there are AgNWs that connect with each other, which ensures a lower Rv value compared to the fabrics modified with the mixture method.
Moreover, the lower values of Rv in relation to Rs for all modified fabrics may be due to the AgNWs filling the spaces between the fibers.
After UV irradiation, the Rs values increase by one order of magnitude for both the AgNWs modified fabrics (Figure 12a). This increase may be caused by the degradation of AgNWs, which is visible in the SEM images as silver precipitates on the surface of the nanowires (Figure 7b and Figure 8b). For the mixture method, the Rs values increase by six orders of magnitude and the fabric becomes non-conductive. For the layer-by-layer method, the Rs value has the same order of magnitude. These differences are related to the different thicknesses of the silanes layer. For the layer-by-layer method, the layer is thicker and protects the AgNWs from the UV radiation. In the case of the mixture method, the silanes coating that covers the AgNWs is thin and does not reflect the UV radiation as efficiently. For fabrics modified with the AgNWs and silanes mixture, the coating is discontinuous and damaged with numerous cavities and cracks (Figure 7c and Figure 8c). This causes interruption percolating paths formed by the AgNWs, which prevent the flow of electrons.
The UV radiation causes an increase in the Rv values for the AgNWs modified fabrics by one order of magnitude (Figure 12b). For the layer-by-layer method, the value only slightly increases. The Rv values of mAr/RF/PD/5Ag+S increase but have the same order of magnitude. For pAr/RF/PD/5Ag+S, an increase by one order of magnitude is observed. The lower increase in Rv compared to Rs after irradiation is due to the fact that AgNWs located between the fibers inside the fabric are less exposed to UV radiation than the AgNWs on its surface.

4. Conclusions

Multifunctional meta- and para-aramid fabrics modified with AgNWs and a mixture of silanes, APTES, and DEDMS, were obtained. The aim of the studies was to protect against UV radiation and improve the mechanical, electrical, and hydrophobic properties of modified aramid fabrics. New functionalization methods, a one-step method (mixture) with AgNWs dispersed in the silanes mixture, and a two-step method (layer-by-layer) in which the silanes mixture was applied on the previously deposited AgNWs layer, were developed.
Fabrics were pre-treated in a low-pressure air RF plasma, and a subsequent polydopamine coating was applied.
The modified fabrics acquired hydrophobic properties. The water contact angle for the meta- and para-aramid fabric was 125° and 120°, respectively, for the mixture and 112° and 114°, respectively, for the layer-by-layer method. The surface free energy for the AgNWs and silanes modified fabrics is lower by about 30% for the meta-aramid fabric and 50% for the para-aramid fabric compared with the reference fabrics.
Better resistance to UV radiation was achieved for the layer-by-layer method. The UV radiation caused no changes in the layer-by-layer coating, while for the mixture coating, there was damage, and some coating fragments were detached. The UV radiation caused a significant decrease in the specific strength of the reference fabrics by about 50% and 60% for the meta- and para-aramid fabric, respectively, while for the mixture and layer-by-layer method, the specific strength values were 71% and 63% higher for the meta-aramid fabric, respectively, and 102% and 110% higher for the para-aramid fabric, respectively. The layer-by-layer modified fabrics were the most abrasion resistant; before and after UV radiation, no thread damage was observed after 100,000 abrasion cycles. The electrical surface resistance for the layer-by-layer method was nine orders of magnitude lower than the reference fabrics, and for the mixture method, it was eight orders of magnitude lower. After UV irradiation, the Rs did not change for the layer-by-layer method and increased by six orders of magnitude for the mixture modified fabrics, which became non-conductive. We selected the layer-by-layer method as the most effective for aramid fabric modification; it results in great surface, electrical, and mechanical properties and better resistance to UV radiation. It protects aramid fabrics from degradation and the deterioration of their functional properties.

Supplementary Materials

The following supporting information can be downloaded at: https://0-www-mdpi-com.brum.beds.ac.uk/article/10.3390/molecules27061952/s1, Figure S1: Images of (a) mAr and (b) pAr fabrics surfaces, before and after UV radiation (365 nm, 96 h), before and after abrasion cycles.

Author Contributions

Conceptualization, A.N., M.C. and G.C.; formal analysis, A.N., M.C. and G.C.; visualization, A.N.; funding acquisition, M.C. and G.C.; investigation, A.N. and M.C.; methodology, A.N., A.B.-K., K.R.-S., I.J. and G.C.; project administration, M.C. and G.C.; writing—original draft, A.N.; writing—review and editing, A.N., M.C. and G.C. All authors have read and agreed to the published version of the manuscript.

Funding

The research was funded by the National Science Center, project grant: 2018/29/B/ST8/02016 and the internal project BZT 0166/2020-2021. The research was carried out within the National Science Center, on the apparatus purchased in the Key Project—POIG.01.03.01-00-004/08 Functional nano and micro textile materials—NANOMITEX and WND-RPLD. 03.01.00-001/09.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

Sample Availability

Samples of the compounds are not available from the authors.

References

  1. Zhang, H.; Liang, G.; Gu, A.; Yuan, L. Facile preparation of hyperbranched polysiloxane-grafted aramid fibers with simulta-neously improved UV resistance, surface activity, and thermal and mechanical properties. Ind. Eng. Chem. Res. 2014, 53, 2684–2696. [Google Scholar] [CrossRef]
  2. Wang, H.; Xie, H.; Hu, Z.; Wu, D.; Chen, P. The influence of UV radiation and moisture on the mechanical properties and micro-structure of single Kevlar fibre using optical methods. Polym. Degrad. Stab. 2012, 97, 1755–1761. [Google Scholar] [CrossRef]
  3. Zhu, J.; Yuan, L.; Guan, Q.; Liang, G.; Gu, A. A novel strategy of fabricating high performance UV-resistant aramid fibers with simultaneously improved surface activity, thermal and mechanical properties through building polydopamine and graphene oxide bi-layer coatings. Chem. Eng. J. 2017, 310, 134–147. [Google Scholar] [CrossRef]
  4. Foksowicz-Flaczyk, J.; Walentowska, J.; Przybylak, M.; Maciejewski, H. Multifunctional durable properties of textile materials modified by biocidal agents in the sol-gel process. Surf. Coat. Technol. 2016, 304, 160–166. [Google Scholar] [CrossRef]
  5. Stoppa, M.; Chiolerio, A. Wearable Electronics and Smart Textiles: A Critical Review. Sensors 2014, 14, 11957–11992. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  6. Gowri, S.; Almeida, L.; Amorim, T.; Carneiro, N.; Souto, A.P.; Esteves, M.F. Polymer nanocomposites for multifunctional fin-ishing of textiles—A review. Text. Res. J. 2014, 80, 1290–1306. [Google Scholar] [CrossRef]
  7. Nejman, A.; Kamińska, I.; Jasińska, I.; Celichowski, G.; Cieślak, M. Influence of Low-Pressure RF Plasma Treatment on Aramid Yarns Properties. Molecules 2020, 25, 3476. [Google Scholar] [CrossRef]
  8. Inagaki, N.; Tasaka, S.; Kawai, H. Surface modification of Kevlar® fiber by a combination of plasma treatment and coupling agent treatment for silicone rubber composite. J. Adhes. Sci. Technol. 1992, 6, 279–291. [Google Scholar] [CrossRef]
  9. Sun, Z.; Zhou, Y.; Li, W.; Chen, S.; You, S.; Ma, J. Preparation of Silver-Plated Para-Aramid Fiber by Employing Low-Temperature Oxygen Plasma Treatment and Dopamine Functionalization. Coatings 2019, 9, 599. [Google Scholar] [CrossRef] [Green Version]
  10. Sa, R.; Yan, Y.; Wei, Z.; Zhang, L.; Wang, W.; Tian, M. Surface Modification of Aramid Fibers by Bio-Inspired Poly(dopamine) and Epoxy Functionalized Silane Grafting. ACS Appl. Mater. Interfaces 2014, 6, 21730–21738. [Google Scholar] [CrossRef]
  11. Chai, D.; Xie, Z.; Wang, Y.; Liu, L.; Yum, Y.-J. Molecular Dynamics Investigation of the Adhesion Mechanism Acting between Dopamine and the Surface of Dopamine-Processed Aramid Fibers. ACS Appl. Mater. Interfaces 2014, 6, 17974–17984. [Google Scholar] [CrossRef] [PubMed]
  12. Zeng, L.; Liu, X.; Chen, X.; Soutis, C. Surface Modification of Aramid Fibres with Graphene Oxide for Interface Improvement in Composites. Appl. Compos. Mater. 2018, 25, 843–852. [Google Scholar] [CrossRef] [Green Version]
  13. Lee, H.; Dellatore, S.M.; Miller, W.M.; Messersmith, P.B. Mussel-Inspired Surface Chemistry for Multifunctional Coatings. Science 2007, 318, 426–430. [Google Scholar] [CrossRef] [Green Version]
  14. Wei, Q.; Zhang, F.; Li, J.; Li, B.; Zhao, C. Oxidant-induced dopamine polymerization for multifunctional coatings. Polym. Chem. 2010, 1, 1430–1433. [Google Scholar] [CrossRef]
  15. Lee, H.; Scherer, N.F.; Messersmith, P.B. Single-molecule mechanics of mussel adhesion. Proc. Natl. Acad. Sci. USA 2006, 103, 12999–13003. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  16. Burzio, L.A.; Waite, J.H. Cross-Linking in Adhesive Quinoproteins: Studies with Model Decapeptides. Biochemistry 2000, 39, 11147–11153. [Google Scholar] [CrossRef] [PubMed]
  17. Sever, M.J.; Weisser, J.T.; Monahan, J.; Srinivasan, S.; Wilker, J.J. Metal-mediated cross-linking in the generation of a ma-rine-mussel adhesive. Angew. Chem. Int. Ed. 2004, 43, 448–450. [Google Scholar] [CrossRef]
  18. Yu, M.; Hwang, J.; Deming, T.J. Role of l-3,4-Dihydroxyphenylalanine in Mussel Adhesive Proteins. J. Am. Chem. Soc. 1999, 121, 5825–5826. [Google Scholar] [CrossRef]
  19. Gu, T.; Zhu, D.; Lu, S. Surface Functionalization of Silver-Coated Aramid Fiber. Polym. Sci. Ser. A 2020, 62, 196–204. [Google Scholar] [CrossRef]
  20. Wang, W.; Li, R.; Tian, M.; Liu, L.; Zou, H.; Zhao, X.; Zhang, L. Surface Silverized Meta-Aramid Fibers Prepared by Bio-inspired Poly(dopamine) Functionalization. ACS Appl. Mater. Interfaces 2013, 5, 2062–2069. [Google Scholar] [CrossRef]
  21. Liu, H.; Zhu, L.; Xue, J.; Hao, L.; Li, J.; He, Y.; Cheng, B. A Novel Two-Step Method for Fabricating Silver Plating Cotton Fabrics. J. Nanomater. 2016, 2016, 2375836. [Google Scholar] [CrossRef] [Green Version]
  22. Sun, Y.; Gates, B.; Mayers, B.; Xia, Y. Crystalline Silver Nanowires by Soft Solution Processing. Nano. Lett. 2002, 2, 165–168. [Google Scholar] [CrossRef]
  23. Wang, Z.; Liu, J.; Chen, X.; Wan, J.; Qian, Y. A Simple Hydrothermal Route to Large-Scale Synthesis of Uniform Silver Nanowires. Chem.—Eur. J. 2004, 11, 160–163. [Google Scholar] [CrossRef] [PubMed]
  24. James, S.; Robinson, A.; Arnold, J.; Worsley, D. The effects of humidity on photodegradation of poly(vinyl chloride) and polyethylene as measured by the CO2 evolution rate. Polym. Degrad. Stab. 2013, 98, 508–513. [Google Scholar] [CrossRef] [Green Version]
  25. Mather, R.R.; Wardman, R.H. The Chemistry of Textile Fibers; RSC Publishing: Cambridge, UK, 2011. [Google Scholar]
  26. Lin, M.C.; Chu, C.J.; Tsai, L.C.; Lin, H.Y.; Wu, C.S.; Wu, Y.P.; Shieh, D.B.; Su, Y.W.; Chen, C.D. Control and Detection of Organosilane Polarization on Nanowire Field-Effect Transistors. Nano Lett. 2007, 7, 3656–3661. [Google Scholar] [CrossRef] [Green Version]
  27. Chiavari, C.; Balbo, A.; Zanotto, F.; Vassura, I.; Bignozzi, M.C.; Monticelli, C. Organosilane coatings applied on bronze: In-fluence of UV radiation and thermal cycles on the protectiveness. Progr. Org. Coat. 2015, 82, 91–100. [Google Scholar] [CrossRef]
  28. Shi, F.; Xu, J.; Zhang, Z. Study on UV-protection and hydrophobic properties of cotton fabric functionalized by graphene oxide and silane coupling agent. Pigment Resin Technol. 2019, 48, 237–242. [Google Scholar] [CrossRef]
  29. Tragoonwichian, S.; O’Rear, E.A.; Yanumet, N. Grafting polymerization of 2-[3-(2h-benzotriazol-2-yl)-4-hydroxyphenyl]ethyl methacrylate on vinyltriethoxysilane-treated cotton for the preparation of ultraviolet-protective fabrics. J. Appl. Polym. Sci. 2009, 114, 62–69. [Google Scholar] [CrossRef]
  30. Roe, B.; Zhang, X. Durable Hydrophobic Textile Fabric Finishing Using Silica Nanoparticles and Mixed Silanes. Text. Res. J. 2009, 79, 1115–1122. [Google Scholar] [CrossRef]
  31. Zeng, X.; Xu, G.; Gao, Y.; An, Y. Surface Wettability of (3-Aminopropyl)triethoxysilane Self-Assembled Monolayers. J. Phys. Chem. B 2010, 115, 450–454. [Google Scholar] [CrossRef]
  32. Zhang, Y.; Shen, Q.; Li, X.; Xie, H.; Nie, C. Facile synthesis of ternary flexible silica aerogels with coarsened skeleton for oil–water separation. RSC Adv. 2020, 10, 42297–42304. [Google Scholar] [CrossRef]
  33. Souza, K.G.D.S.; Cotting, F.; Aoki, I.V.; Amado, F.D.R.; Capelossi, V.R. Study of the wettability and the corrosion protection of the hybrid silane (3-aminopropyl) triethoxysilane (APTES) and (3-glycidyloxypropyl) trimethoxysilane (GPTMS) film on galvannealed steel. Matéria 2020, 25. [Google Scholar] [CrossRef]
  34. Hasanzadeh, M.; Far, H.S.; Haji, A.; Rosace, G. Facile fabrication of breathable and superhydrophobic fabric based on silica na-noparticles and amino-modified polydimethylsiloxane. Preprints 2020, 257, 5491–5498. [Google Scholar]
  35. Liu, H.; Lee, Y.-Y.; Norsten, T.B.; Chong, K. In situ formation of anti-bacterial silver nanoparticles on cotton textiles. J. Ind. Text. 2013, 44, 198–210. [Google Scholar] [CrossRef]
  36. Giesz, P.; Mackiewicz, E.; Nejman, A.; Celichowski, G.; Cieślak, M. Investigation on functionalization of cotton and viscose fabrics with AgNWs. Cellulose 2016, 24, 409–422. [Google Scholar] [CrossRef] [Green Version]
  37. Schmidt, H.; Witkowska, B.; Kamińska, I.; Twarowska-Schmidt, K.; Wierus, K.; Puchowicz, D. Comparison of the rates of polypropylene fibre degradation caused by artificial light and sunlight. Fib. Tex. East. Eur. 2011, 4, 53–58. [Google Scholar]
  38. Owens, D.K.; Wendt, R.C. Estimation of the surface free energy of polymers. J. Appl. Polym. Sci. 1969, 13, 1741–1747. [Google Scholar] [CrossRef]
  39. Cieslak, M.; Puchowicz, D.; Schmidt, H. Evaluation of the possibility of using surface free energy study to design protective fabrics. Text. Res. J. 2011, 82, 1177–1189. [Google Scholar] [CrossRef]
  40. Giesz, P.; Celichowski, G.; Puchowicz, D.; Kamińska, I.; Grobelny, J.; Batory, D.; Cieślak, M. Microwave-assisted TiO2: Anatase formation on cotton and viscose fabric surfaces. Cellulose 2016, 23, 2143–2159. [Google Scholar] [CrossRef] [Green Version]
  41. Schmidt, H.; Cieślak, M. Concrete with carpet recyclates: Suitability assessment by surface energy evaluation. Waste Manag. 2008, 28, 1182–1187. [Google Scholar] [CrossRef]
  42. Sabdin, S.; Azmi, M.A.M.; Badruzaman, N.A.; Makmon, F.Z.; Aziz, A.A.; Said, N.A.M. Effect of APTES Percentage towards Reduced Graphene Oxide Screen Printed Electrode Surface for Biosensor Application. Mater. Today Proc. 2019, 19, 1183–1188. [Google Scholar] [CrossRef]
  43. Jiang, J.; Zhu, L.; Zhu, L.; Zhang, H.; Zhu, B.; Xu, Y. Antifouling and Antimicrobial Polymer Membranes Based on Bioinspired Polydopamine and Strong Hydrogen-Bonded Poly(N-vinyl pyrrolidone). ACS Appl. Mater. Interfaces 2013, 5, 12895–12904. [Google Scholar] [CrossRef] [PubMed]
  44. Chen, S.; Zhang, L.; Sun, M.; Zhang, X.; Chen, W. Surface modification of polypropylene nonwoven fabrics by grafting of polydopamine. Adv. Polym. Technol. 2018, 37, 3519–3528. [Google Scholar] [CrossRef] [Green Version]
  45. Zhang, Y.; Bai, S.; Chen, T.; Yang, H.; Guo, X. Facile preparation of flexible and highly stable graphene oxide-silver nanowire hybrid transparent conductive electrode. Mater. Res. Express 2019, 7, 016413. [Google Scholar] [CrossRef] [Green Version]
Figure 1. The scheme of the modification of aramid fabrics with (a) low-pressure air RF plasma and polydopamine and (b) the application of AgNWs and silanes by the mixture and layer-by-layer method.
Figure 1. The scheme of the modification of aramid fabrics with (a) low-pressure air RF plasma and polydopamine and (b) the application of AgNWs and silanes by the mixture and layer-by-layer method.
Molecules 27 01952 g001
Figure 2. SEM images of (a) reference, (b) plasma treated, and (c) polydopamine modified mAr fibers (magnification of 10,000×).
Figure 2. SEM images of (a) reference, (b) plasma treated, and (c) polydopamine modified mAr fibers (magnification of 10,000×).
Molecules 27 01952 g002
Figure 3. SEM images of (a) reference, (b) plasma treated, and (c) polydopamine modified pAr fibers (magnification of 10,000×).
Figure 3. SEM images of (a) reference, (b) plasma treated, and (c) polydopamine modified pAr fibers (magnification of 10,000×).
Molecules 27 01952 g003
Figure 4. FTIR spectrum of polydopamine, reference, and RF plasma and polydopamine functionalized para-aramid fabrics in the range of (a) 600–1750 cm−1 and (b) 2400–4000 cm−1.
Figure 4. FTIR spectrum of polydopamine, reference, and RF plasma and polydopamine functionalized para-aramid fabrics in the range of (a) 600–1750 cm−1 and (b) 2400–4000 cm−1.
Molecules 27 01952 g004
Figure 5. SEM images of modified mAr fibers after the (a) 1-fold and (b) 5-fold application of AgNWs and the (c) mixture Ag+S, and (d) layer-by-layer Ag/S modification (magnification of 2500× and 20,000×).
Figure 5. SEM images of modified mAr fibers after the (a) 1-fold and (b) 5-fold application of AgNWs and the (c) mixture Ag+S, and (d) layer-by-layer Ag/S modification (magnification of 2500× and 20,000×).
Molecules 27 01952 g005
Figure 6. SEM images of modified pAr fibers after the (a) 1-fold and (b) 5-fold application of AgNWs and the (c) mixture Ag+S, and (d) layer-by-layer Ag/S modification (magnification of 2500× and 20,000×).
Figure 6. SEM images of modified pAr fibers after the (a) 1-fold and (b) 5-fold application of AgNWs and the (c) mixture Ag+S, and (d) layer-by-layer Ag/S modification (magnification of 2500× and 20,000×).
Molecules 27 01952 g006
Figure 7. SEM images of UV irradiated (365 nm, 96 h) mAr fibers (a) reference and after (b) 5-fold AgNWs application, (c) mixture Ag+S and (d) layer by layer Ag/S modification (magnification of 6500× and 20,000×).
Figure 7. SEM images of UV irradiated (365 nm, 96 h) mAr fibers (a) reference and after (b) 5-fold AgNWs application, (c) mixture Ag+S and (d) layer by layer Ag/S modification (magnification of 6500× and 20,000×).
Molecules 27 01952 g007
Figure 8. SEM images of UV irradiated (365 nm, 96 h) pAr fibers (a) reference and after (b) 5-fold AgNWs application, (c) mixture Ag+S, and (d) layer-by-layer Ag/S modification (magnification of 6500× and 20,000×).
Figure 8. SEM images of UV irradiated (365 nm, 96 h) pAr fibers (a) reference and after (b) 5-fold AgNWs application, (c) mixture Ag+S, and (d) layer-by-layer Ag/S modification (magnification of 6500× and 20,000×).
Molecules 27 01952 g008
Figure 9. Surface free energy (γs) of unmodified and modified mAr (a) and pAr (b) fabrics (γsd—dispersive component, γsp—polar component).
Figure 9. Surface free energy (γs) of unmodified and modified mAr (a) and pAr (b) fabrics (γsd—dispersive component, γsp—polar component).
Molecules 27 01952 g009
Figure 10. Specific strength of unmodified and modified mAr (a) and pAr (b) fabrics before and after UV irradiation (365 nm, 96 h).
Figure 10. Specific strength of unmodified and modified mAr (a) and pAr (b) fabrics before and after UV irradiation (365 nm, 96 h).
Molecules 27 01952 g010
Figure 11. Results of the Martindale’s abrasion test for unmodified and modified mAr (a) and pAr (b) fabrics before and after UV irradiation (365 nm, 96 h).
Figure 11. Results of the Martindale’s abrasion test for unmodified and modified mAr (a) and pAr (b) fabrics before and after UV irradiation (365 nm, 96 h).
Molecules 27 01952 g011
Figure 12. Electrical surface resistance (Rs) (a) and electrical volume resistance (Rv) (b) of unmodified and modified mAr and pAr fabrics before and after UV irradiation (365 nm, 96 h).
Figure 12. Electrical surface resistance (Rs) (a) and electrical volume resistance (Rv) (b) of unmodified and modified mAr and pAr fabrics before and after UV irradiation (365 nm, 96 h).
Molecules 27 01952 g012
Table 1. Mass per unit area of the reference and modified aramid fabrics.
Table 1. Mass per unit area of the reference and modified aramid fabrics.
FabricMass per Unit Area,
g/m2
Mass per Unit Area of AgNW Coating,
g/m2
Mass per Unit Area of Silanes Coating,
g/m2
Mass per Unit Area of AgNWs and Silanes Coating,
g/m2
mAr205 ± 2
mAr/RF/PD/1Ag214 ± 69 ± 3
mAr/RF/PD/5Ag248 ± 743 ± 2
mAr/RF/PD/5Ag+S273 ± 7 68 ± 5
mAr/RF/PD/5Ag/S305 ± 943 ± 262 ± 1105 ± 3
pAr165 ± 3
pAr/RF/PD/1Ag171 ± 46 ± 1
pAr/RF/PD/5Ag200 ± 135 ± 3
pAr/RF/PD/5Ag+S222 ± 5 57 ± 2
pAr/RF/PD/5Ag/S263 ± 435 ± 363 ± 598 ± 6
Table 2. Characteristics of standard liquids.
Table 2. Characteristics of standard liquids.
LiquidSurface Tension, mJ/m2
γlγldγlp
Water (distilled)72.821.851.0
Formamide (99.5%, Sigma-Aldrich, UK)58.039.019.0
Diiodomethane (99%, Sigma-Aldrich, UK)50.848.52.3
Table 3. FTIR bands assigned for the pAr fabric and the reference polydopamine film.
Table 3. FTIR bands assigned for the pAr fabric and the reference polydopamine film.
pAr FabricReference Polydopamine Film
Bands, cm−1Description [7,10,34]Bands, cm−1Description [7,10,34]
698C–H out of plane substituted aromatic ring698C–H out of plane substituted aromatic ring
821p-substituted phenyl911CONH bending, C–N stretching
1306C–N stretching1034C–O stretching
1509C=C stretching1113C–H bending
1538N–H bending1335C–N stretching
1637C=O stretching1413C=O stretching
1740C=O stretching1440C=C stretching vibrations of an aromatic ring
3323N–H stretching1527C=N stretching vibrations of an aromatic ring
1594C=C stretching vibrations of an aromatic ring, C–N stretching
3150N–H stretching
Table 4. The mean values of the weight percentages of the elements with standard deviations for unmodified and modified mAr and pAr fabrics.
Table 4. The mean values of the weight percentages of the elements with standard deviations for unmodified and modified mAr and pAr fabrics.
FabricWeight Percentage of Elements, wt.%
CNOSiAg
mAr 168 ± 110 ± 121 ± 1
mAr/RF/PD/1Ag 268 ± 18 ± 120 ± 1 3 ± 1
mAr/RF/PD/5Ag 256 ± 27 ± 118 ± 1 18 ± 2
mAr/RF/PD/5Ag+S 254 ± 16 ± 128 ± 15 ± 16 ± 1
mAr/RF/PD/5Ag/S 241 ± 18 ± 131 ± 17 ± 112 ± 1
pAr 166 ± 113 ± 119 ± 1
pAr/RF/PD/1Ag 1,266 ± 16 ± 120 ± 1 6 ± 1
pAr/RF/PD/5Ag 1,254 ± 35 ± 118 ± 1 21 ± 3
pAr/RF/PD/5Ag+S 1,254 ± 15 ± 126 ± 15 ± 18 ± 1
pAr/RF/PD/5Ag/S 1,242 ± 17 ± 131 ± 16 ± 112 ± 1
1 The total weight percentage of the elements is less than 100 wt.% because of the trace amounts of Na and S (S only for the pAr fabric), which are less than 1 wt.% and are not included in Table 2. In the case of mAr, the presence of Na is due to the technology of fiber production as a result of the reaction of two comonomers in tetrahydrofuran. An oligomer suspension is formed, which combines with sodium carbonate, and fibers are formed [7,25]. In turn, pAr fibers are produced by the condensation of 1,4-diaminobenzene and terephthaloyl chloride. The formed pAr is immersed in sulfuric acid, and then sodium hydroxide is added for neutralization. The product of neutralization is sodium sulphate [7,25]. 2 For all AgNWs modified fabrics, the trace amounts of Cl (<1 wt.%), which came from silver chloride as a by-product of the AgNWs colloid synthesis, were present and are not included in Table 2.
Table 5. Contact angles of water (ΘW), formamide (ΘF), and diiodomethane (ΘDIM) for unmodified and modified mAr and pAr fabrics.
Table 5. Contact angles of water (ΘW), formamide (ΘF), and diiodomethane (ΘDIM) for unmodified and modified mAr and pAr fabrics.
FabricContact Angle [o]
ΘWΘFΘDIM
mAr64 ± 258 ± 263 ± 2
mAr/RF19 ± 336 ± 327 ± 3
mAr/RF/PD0 ± 036 ± 190 ± 0
mAr/RF/PD/1Ag77 ± 274 ± 336 ± 4
mAr/RF/PD/5Ag87 ± 190 ± 232 ± 3
mAr/RF/PD/5Ag+S125 ± 5106 ± 255 ± 2
mAr/RF/PD/5Ag/S112 ± 296 ± 251 ± 1
pAr77 ± 433 ± 214 ± 3
pAr/RF12 ± 518 ± 55 ± 1
pAr/RF/PD0 ± 019 ± 168 ± 1
pAr/RF/PD/1Ag84 ± 477 ± 236 ± 3
pAr/RF/PD/5Ag89 ± 385 ± 234 ± 4
pAr/RF/PD/5Ag+S120 ± 1106 ± 358 ± 2
pAr/RF/PD/5Ag/S114 ± 2100 ± 153 ± 1
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Nejman, A.; Baranowska-Korczyc, A.; Ranoszek-Soliwoda, K.; Jasińska, I.; Celichowski, G.; Cieślak, M. Silver Nanowires and Silanes in Hybrid Functionalization of Aramid Fabrics. Molecules 2022, 27, 1952. https://0-doi-org.brum.beds.ac.uk/10.3390/molecules27061952

AMA Style

Nejman A, Baranowska-Korczyc A, Ranoszek-Soliwoda K, Jasińska I, Celichowski G, Cieślak M. Silver Nanowires and Silanes in Hybrid Functionalization of Aramid Fabrics. Molecules. 2022; 27(6):1952. https://0-doi-org.brum.beds.ac.uk/10.3390/molecules27061952

Chicago/Turabian Style

Nejman, Alicja, Anna Baranowska-Korczyc, Katarzyna Ranoszek-Soliwoda, Izabela Jasińska, Grzegorz Celichowski, and Małgorzata Cieślak. 2022. "Silver Nanowires and Silanes in Hybrid Functionalization of Aramid Fabrics" Molecules 27, no. 6: 1952. https://0-doi-org.brum.beds.ac.uk/10.3390/molecules27061952

Article Metrics

Back to TopTop