Next Article in Journal
Review: Local Tumor Necrosis Factor-α Inhibition in Inflammatory Bowel Disease
Next Article in Special Issue
Development of a Nonwoven Hemostatic Dressing Based on Unbleached Cotton: A De Novo Design Approach
Previous Article in Journal
pH-Sensitive Folic Acid Conjugated Alginate Nanoparticle for Induction of Cancer-Specific Fluorescence Imaging
Previous Article in Special Issue
Growth Factors Delivery System for Skin Regeneration: An Advanced Wound Dressing
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

A Novel Composite Hydrogel Composed of Formic Acid-Decellularized Pepsin-Soluble Extracellular Matrix Hydrogel and Sacchachitin Hydrogel as Wound Dressing to Synergistically Accelerate Diabetic Wound Healing

1
School of Pharmacy, College of Pharmacy, Taipei Medical University, 250 Wu-Hsing Street, Taipei 11031, Taiwan
2
Department of Surgery, School of Medicine, College of Medicine, Taipei Medical University, 250 Wu-Hsing Street, Taipei 11031, Taiwan
3
Division of General Surgery, Department of Surgery, Taipei Medical University Hospital, 252 Wu-Hsing Street, Taipei 11031, Taiwan
*
Authors to whom correspondence should be addressed.
Submission received: 29 April 2020 / Revised: 6 June 2020 / Accepted: 9 June 2020 / Published: 11 June 2020
(This article belongs to the Special Issue Advances in Wound Dressings and Materials)

Abstract

:
Extracellular matrix (ECM) hydrogel can create a favorable regenerative microenvironment and act as a promising dressing for accelerating the healing of diabetic wound. In this study, a simple and effective decellularization technique was developed and optimized to obtain acellular extracellular matrix (aECM) from porcine skin. It was found that decellularization at 30% formic acid for 72 h effectively decellularized porcine skin while retaining >75% collagen and ~37% GAG in the aECM with no presence of nuclei of cellular remnants. aECM hydrogel was fabricated by digesting aECM with pepsin in various acidic solutions (0.1 N HCl, glycolic acid (GA) and 2-pyrrolidone-5-carboxylic acid (PCA)) and then treated with a pH-controlled neutralization and temperature-controlled gelation procedure. Based on physical characterizations, including SDS-PAGE, rheological analysis and SEM analysis, aECMHCl hydrogels fabricated at 25 mg/mL in 0.1 N HCl were selected. Four polymeric ECM-mimic hydrogels, including sacchachitin (SC), hyaluronic acid (HA) and chitosan (CS) and three composite hydrogels of combining SC either with aECMHCl,25 (aECMHCl/SC), HA (HA/SC) or CS (SC/CS) were prepared and evaluated for WS-1 cell viability and wound-healing effectiveness. Cell viability study confirmed that no hydrogel dressings possessed any toxicity at all concentrations examined and ECMHCl, HA and ECMHCl/SC at higher concentrations (>0.05%) induced statistically significant proliferation. Diabetic wound healing study and histological examinations revealed that ECMHCl/SC hydrogel was observed to synergistically accelerate wound healing and ultimately stimulated the growth of hair follicles and sweat glands in the healing wound indicating the wound had healed as functional tissues. The results support the great potential of this newly produced ECMHCl/SC composite hydrogel for healing and regeneration of diabetic wounds.

Graphical Abstract

1. Introduction

Extracellular matrix (ECM) is the largest component of normal skin and ECM synthesis is crucial for wound healing [1]. ECM components include collagen, proteoglycans, such as glycosaminoglycan (GAG), hyaluronic acid (HA) and so forth. [2]. ECM lacks immunogenicity and its biological properties are superior to other types of dressings. Since that, many studies have demonstrated that ECM can act as a dressing creating a favorable regenerative microenvironment for repairing wounds [3]. Nevertheless, it is difficult to construct a wound dressing with the same composition as that of in vivo ECM. Consequently, decellularization of biological tissues has become an attractive strategy for obtaining ECM. The requirements for ECM after decellularization are an acceptable amount of residual DNA (<50 ng DNA per mg dry weight), preservation of the collagen component (about 75%) and retention of the ECM structure [4]. To improve the efficiency of decellularization, enzymatic, chemical and physical methods were developed for different types of tissue and species of origin [5,6,7]. Enzymatic methods for decellularization usually use proteases and chelating agents (such as ethylenediaminetetraacetic acid (EDTA)). The methods can effectively remove cellular materials and preserve the collagen components but they might disrupt the ECM structure [8], a length incubation was necessitated [9] or with impractical device to assist [10]. Chemical methods by acidic and alkaline treatments can solubilize the cellular cytoplasmic components, remove nucleic acids (for instance, DNA), preserve the structure and function of the native ECM and simultaneously disinfect the material through entering microorganisms and oxidizing microbial enzymes [11]. A simple formic acid treatment able to remove most of the cellular contents and preserve the highest ECM contents in the decellularized porcine menisci was reported by Chen et al. [12]. Physical methods can be used to decellularize tissues by disrupting cellular membranes but cellular debris cannot be removed. Therefore, physical methods are usually combined with chemical or enzymatic treatment [13,14]. Overall, it was inevitable to develop simple, effective and optimized decellularization techniques to obtain ECM from porcine skin for wound-healing medical applications.
The “wet wound healing theory” proposes that the wet healing environment is favorable to the granulation growth and to the enablement of the skin cell division, thereby promoting the complete wound healing [15]. Based on this theory, intrinsic characteristics of hydrogels or pastes are expectable to be advantageous for the wound healing process since they provide the dressing with desirable essential properties—better biocompatibility; protection from physical injury; optimal gaseous exchange and nutrients supply to cells due to high sponginess; additionally, their swellability allows for the absorption of excess exudates as well as the maintenance of an optimal moisture environment around the wound, which exhibited to accelerate the wound re-epithelialization process [16]. Hydrogels or pastes based on the natural polymers chitosan [17] and hyaluronic acid [18], an interpenetrated polymer network (IPN) composed of chitosan/oxidized hyaluronic acid/catechol terpolymer/Fe [16], pepsin-soluble collagen isolated from Nile Tilapia skin [15], micronized ADM [19], have been explored for this purpose and demonstrated to provide an extracellular matrix (ECM) mimicking microenvironment with high cell affinity and bioactive functionalities that could enhance the tissue regeneration process and has a great potential for its application as wound dressing.
Furthermore, ECM hydrogels have also been created from numerous tissue sources in almost every organ system and used to facilitate functional and constructive tissue remodeling in a variety of clinical applications, such as ischemic injuries and organ regeneration or replacement [20]. There are two key steps in the fabrication of ECM hydrogels from acellular ECM (aECM)—solubilization of aECM and temperature- and/or pH-controlled neutralization [21]. The most popular method to solubilize aECM is to digest it in pepsin with acetic acid or dilute hydrochloric acid for different times [22,23]. The type of acidic solution and digestion time used are tailored to produce different bioactive properties for each clinical application. Then pepsin-soluble aECM is treated with pH-controlled neutralization and temperature-controlled gelation procedures and manipulated to form aECM hydrogels [24,25]. Furthermore, it has been reported by Guo et al. that aECM may accelerate the healing velocity of uninfected, non-ischemic, full-thickness diabetic foot ulcer with showing superiority and generating no more complications compared with standard of care alone [26]. Since there are abundant porcine skin resources, it was thought that aECM as a hydrogel form might be fabricated from acellular ECM obtained by decellularizing porcine skin for utilization as wound dressing to enhance the healing of diabetic wounds. In this study, therefore, a simple and effective method to decellularize porcine skin with formic acid treatment followed that reported by our labs [12] was developed and optimized, which was then further processed to produce aECM hydrogels by pepsin digestion and pH-controlled neutralization and temperature-controlled gelation procedures. The extent of decellularization and major ECM components (collagen and glycosaminoglycan) remained were characterized. Moreover, the sol-gel transition was measured and a rheological analysis of the obtained aECM hydrogels was conducted. In addition, hydrogels based on the natural polymers sacchachitin (SC) [27], chitosan (CS) [17] and hyaluronic acid (HA) [18] that able to provide an extracellular matrix (ECM) mimicking microenvironment and their composite hydrogels were included for comparison in in vitro cell viability of WS-1 human skin fibroblasts and the wound healing effectiveness on diabetic wound model of rat.

2. Materials and Methods

Acetone was purchased from ECHO Chemical (Miaoli, Taiwan). Sodium chloride (NaCl) and sodium hydroxide (NaOH) were obtained from Showa Chemical (Tokyo, Japan). Citric acid, sodium citrate, trypsin, pepsin, formic acid, 10% formaldehyde, glycolic acid, 2-pyrrolidone-5-carboxylic acid (PCA), papain, l-Cysteine hydrochloride, sodium EDTA, Trizma® base, sodium dodecyl sulfate (SDS), glycerol, 2-mercaptoethanol, bromophenol blue, methanol, acetic acid, coomassie blue R-250, chitosan (CS, with a molecular weight of 50–190 kD and 75–85% extent of deacetylation) and nicotinamide (Vit.B3) were purchased from Sigma-Aldrich (St. Louis, MO, USA). Hydroxyproline kit and glycosaminoglycan (GAG) kit were supplied by Chondrex (Redmond, WA, USA). Phosphate buffered saline (PBS) and penicillin streptomycin (PS) were purchased from Corning (Corning, NY, USA). Hydrochloric acid (HCl) and triethanolamine (TEA) were obtained from Merck (Darmstadt, Germany). Protein marker was purchased from BioTools (New Taipei, Taiwan) and 30% acrylamide/bis solution (37.5:1), tetramethylethylenediamine (TEMED), ammonium persulfate (APS) and glycine were obtained from Bio-Rad (Hercules, CA, USA). Porcine type I collagen standard-FlexiCol® was purchased from advanced BioMatrix (San Diego, CA, USA). Hydroxyethyl Cellulose (HEC, Natrosol 250 HHX Pharm) was supplied by Ashland LLC (Covington, KY, USA). Hyaluronic acid (HA)-Freda® was obtained from Bloomage Freda Biopharm (Jinan, China). Sacchachitin (SC, 2% w/v hydrogel obtained by mechanical disintegration of sacchachitin microfiber in ddH2O as that reported previously [27]). Minimum essential medium (MEM), fetal bovine serum (FBS) and a picoGreen quantification kit were purchased from Thermo Fisher Scientific (Waltham, MA, USA). WST-1 cell proliferation reagent was obtained from Roche Diagnostics GmBH (Mannheim, Germany). Streptozotocin (STZ) was purchased from ChemCruz® (Santa Cruz, CA, USA). Anti-CD31 antibody was obtained from Abcam (Cambridge, UK).

2.1. Development of a Decellularization Method for Porcine Skin

Porcine skin was obtained from a slaughterhouse in Taiwan and washed with water. Its outer and inner surfaces were scraped to remove hair and subcutaneous fat and then the skin was cut into pieces (7 × 5 cm2). In order to remove all of the fat, these pieces were soaked in acetone for 72 h. Then, the acetone was decanted and the pieces were cleaned with deionized water and subsequently treated with 10% sodium chloride at 4 °C for 24 h. The sodium chloride solution was decanted and the pieces were washed again with deionized water. Salt-free pieces of tissue were soaked in 1.92% citrate buffer (pH 4.3) at 25 °C for 48 h [28,29]. The swollen tissues obtained after soaking in citrate buffer were immersed for 18 h in a 0.25% trypsin solution at 25 °C. Then, they were repeatedly washed with phosphate buffer and cut into small pieces (0.5 × 0.2 cm). These small pieces were agitated at 120 rpm with different concentrations (10%, 20% and 30%) of formic acid for different times (24, 48 and 72 h). Finally, these decellularized skin were washed thorough with phosphate buffer until neutral and then lyophilized to obtain aECM samples. They were stored in a desiccator until use.

2.2. Evaluation of the Decellularization Efficiency

2.2.1. Histological Analysis

First, the decellularization efficiencies of aECM treated with different formic acid concentrations (10%, 20% and 30%) for different times (24, 48 and 72 h) were verified by histological staining. Specimens were fixed in 10% (v/v) neutral buffered formalin for 18 h and embedded in paraffin. Untreated porcine skin served as a control group. These specimens were cut into 5~10-µm thicknesses and stained with hematoxylin and eosin (H&E) to inspect fibroblast cells (stained bluish-purple by hematoxylin) and collagen fibers (stained pink by eosin) under an Olympus BX43 stereomicroscope (Olympus, Tokyo, Japan).

2.2.2. Biochemical Analysis

To measure amounts of DNA, GAG and total collagen remaining after decellularization, aECM samples were first digested with a papain solution at 60 °C for 16 h. Quantitation of DNA was carried out using a PicoGreen DNA detection kit (Thermo Fisher Scientific, Waltham, MA, USA). The fluorescence intensity was measured with a Cytation™ 3 cell imaging multi-mode reader (Bio-Tek, Winooski, VT, USA) at an excitation wavelength of 480 nm and emission at 520 nm. The fluorescence of the DNA-free blank was subtracted from that of the experimental groups to account for the fluorescence of the sample alone. In general, hydroxyproline was used to determine the collagen content. Amounts of hydroxyproline and GAG were respectively determined with a hydroxyproline assay kit (# 6017) and GAG kit (# 6022; Chondrex, Redmond, WA, USA) according to the manufacturer’s instructions. The absorbance against a background control was detected at respective wavelengths of 525 and 530 nm with a Cytation™ 3 cell imaging multi-mode reader. Then, the hydroxyproline content was converted to that of total collagen using a mass ratio of 7.41.

2.3. Preparation and Process Optimization of aECM Hydrogels

According to the criteria of decellularization efficiency (acceptable amounts of residual DNA after decellularization of <50 ng DNA per mg dry weight), an optimized aECM was selected from the above experiment for use in the following hydrogel preparation and process optimization. Different weights of optimized aECM (at either 10, 25 or 50 mg/mL) were digested with a solution of 1 mg/mL porcine pepsin in different acidic solutions (0.1 N HCl, glycolic acid (GA) and 2-pyrrolidone-5-carboxylic acid (PCA), designated as aECMHCl, aECMGA and aECMPCA, respectively) under a constant stirring rate (400 rpm) for 48 h at 25 °C. The acronym of these samples is listed in Table 1. Subsequently, gelation was induced by neutralizing the pH value to 7 with 2 N NaOH and heating to 37 °C. After that, the aECM hydrogels were formed and were characterized.

2.4. Characterization of aECM Hydrogels

2.4.1. Sol-Gel Phase Transition

Effects of different concentrations of aECM digested with the same pepsin concentration in different acidic solution on the sol-gel status of hydrogels were evaluated using test tube inversion in a 15-mL test tube at 25 and 37 °C followed the same procedure as previously reported [30].

2.4.2. Rheological Studies of aECM Hydrogels

Since it was found that aECM fabricated at 25 mg/mL in three acidic solutions examined was able to transform to gel or gel-like, rheological characteristics of aECMHCl,25, aECMGA,25 and aECMPCA,25 hydrogels were examined with a rheometer (HAAKE™ Rotation Rheometer RS-1; Thermo Fisher Scientific, Waltham, MA, USA) using the oscillatory shear stress method followed the same procedure as previously reported [29]. The linear viscoelastic region (LVR) of a hydrogel was determined and the storage modulus (G′) and loss modulus (G″) values were compared under the same physical conditions while holding the frequency (1 Hz) constant and increasing the stress strain from 0.1 to 100 Pa and holding the temperature at either 25 or 37 °C. The rheological behavior of the aECMHCl,25+SC hydrogel dressing was evaluated as well using the same method as described above.

2.4.3. Scanning Electron Microscopy (SEM)

For SEM (Hitachi, SU3500, Tokyo, Japan), freeze-dried aECMHCl,25, aECMGA,25, aECMPCA,25 and aECMHCl,25+SC sponges fabricated at 25 mg/mL were mounted with conductive carbon tape, sputter-coated with gold (Hitachi IB-2) and imaged on a Hitachi SU3500 SEM (Tokyo, Japan) at a 5-mm working distance and an accelerating voltage of 2.5 kV.

2.4.4. Qualitative Analysis of Collagen in aECM Hydrogels

For a qualitative analysis of collagen in aECM hydrogels, sodium dodecylsulfate (SDS)-polyacrylamide gel electrophoresis (PAGE) was carried out, using 5% (w/v) polyacrylamide (Bio-Rad, Hercules, CA, USA) for the separating gel and 4% (w/v) polyacrylamide for the stacking gel. The aECMHCl,25, aECMGA,25 and aECMPCA,25 hydrogels and a standard (porcine type I collagen, FlexiCol®) were prepared in 0.5 M Tris-HCl buffer (pH 6.8) containing 10% SDS, 30% glycerol, 1% 2-mercaptoethanol and 0.02% bromophenol blue and then heated to 95 °C for 5 min. Next, 8 µL of a protein marker (BioTools, New Taipei City, Taiwan), 30 µL of the standard and 30 µL of the three hydrogels were loaded and electrophoresed at 85~100 V on vertical slab gels until the bromophenol blue had moved out of the gel. Polyacrylamide gels were stained for 2 h with 0.1% Coomassie blue R-250 in acetic acid/methanol/water 2:5:5 (v/v/v) and were destained in 7.5% acetic acid/15% methanol.

2.5. Fabrication and In Vitro Cell Viability Test of Hydrogel Dressings

There listed formulations for five kinds of hydrogel dressings and three kinds of composite hydrogels in Table 2 that was subjected to evaluate the effectiveness for wound healing. Five kinds of hydrogel dressings including HEC, CS, SC, HA and aECMHCl,25 were fabricated simply by dissolving the indicated amount in the designated solvent and three kinds of composite hydrogel including aECMHCl,25/SC, HA/SC and CS/SC were prepared simply by mixing two hydrogel components together. These hydrogel dressings were prepared and then subjected to UV radiation for sterilization.
WS1 human skin fibroblasts (American Type Culture Collection, Manassas, VA, USA) were maintained in α-minimum essential media (MEM) (Thermo Fisher Scientific, Waltham, MA, USA) with 10% fetal bovine serum (FBS, Thermo Fisher Scientific) and 1% penicillin-streptomycin (Level Biotechnology, New Taipei City, Taiwan) at 37 °C with 5% CO2. Cells were seeded at a density of 104 cells/well in 96-well plates. Different concentrations (0.005%, 0.01%, 0.05%, 0.1% and 0.5% w/v) of eight kinds of sterilized hydrogel dressings were added to each well. After 72 h of incubation, 10 µL of WST-1 reagent was added to each well and incubation continued at 37 °C with 5% CO2 for additional 3 h. Cell viability was measured using the WST-1 cell proliferation reagent (Roche Diagnostics, Mannheim, Germany). In principle, the tetrazolium salt WST-1 (4-[3-(4-Iodophenyl)-2-(4-nitro-phenyl)-2H-5-tetrazolio]-1,3-benzene disulfonate) was cleaved to a soluble formazan by mitochondrial dehydrogenase in viable cells. The proliferation of viable cells leads to an increased overall activity of these enzymes. Corresponding changes in absorbance of the dye solution were detected at a wavelength 440 nm with a Cytation™ 3 cell imaging multi-mode reader.

2.6. Wound-Healing Studies

2.6.1. Diabetic Rats in Wound-Healing Studies

All animal experiments were performed in specific pathogen-free conditions with a protocol (no. LAC-2017-0352, 2017/12/08–2020/12/07) approved by the Laboratory Animal Center of Taipei Medical University (Taipei, Taiwan). Animal study design, requirements of laboratory animals and selection of types and number of animals have also been justified with adhering to the 3Rs principles (replacement, reduction and refinement). Sprague-Dawley rats (males, 8 weeks old) were obtained from BioLASCO Taiwan (Taipei, Taiwan) and housed under a 12-h light/dark cycle, allowed food and water ad libitum and acclimatized for 1 week before the experiment. Diabetes was induced in these rats by an intravenous (i.v.) injection of a solution of 65 mg/kg streptozocin (Santa Cruz Biochemicals, Santa Cruz, CA, USA) [31]. Blood glucose values were measured with a Roche® ACCU-CHEK® Performa blood-glucose meter (Roche®, Taipei, Taiwan) and weights were also recorded. After 7 days, if blood glucose values were >200 mg/dL, rats were considered to be diabetic. The diabetic rats were anesthetized with Zoleti® (VIRBAC, Carros, France) and were used to study the wound-healing rate. The dorsal hair of a rat was removed with an electric razor. Four wounds of equal area were created with an 8-mm biopsy punch and silicon splints were put in place to prevent wound deformation and contraction. Each wound was randomly covered with an equal-sized hydrogel dressing, including one control (HEC), three hydrogels (SC, HA and CS) based on the natural polymers of sacchachitin (SC), chitosan (CS) and hyaluronic acid (HA) that are able to provide an extracellular matrix (ECM) mimicking microenvironment, aECMHCl,25 hydrogel dressings and three kinds of composite hydrogels (aECMHCl,25/SC, HA/SC and CS/SC). Hydrogel dressings were applied on days 0, 2, 4, 6, 8, 10, 12, 14 and 16 and meanwhile, the remaining wound area was measured by analyzing photographs using a digital camera. Images were analyzed with ImageJ software (NIH). The wound closure rate was evaluated. Blood glucose values and weights were also monitored.

2.6.2. Histological Analysis

On days 8 and 14, wounds covered with dressings were sectioned, fixed in 10% (w/v) neutral buffered formalin, dehydrated through an ethanol series and embedded in paraffin. The embedded specimen of 5~10 µm in thickness were stained with hematoxylin and eosin (H&E) to visualize nuclei or stained with Masson’s trichrome (MT) for collagen or stained with an anti-cluster of differentiation 31 (CD31) antibody (ab182981, Abcam, Cambridge, UK) to observe the growth status of microvascular tissues. All samples were evaluated under optical microscopy (BX41, Olympus, Tokyo, Japan).

3. Results and Discussion

3.1. Evaluation of the Decellularization Efficiency

In our preliminary studies showed that citric acid and malic acid treatments of porcine skin were insufficient and not ideal decellularization reagents to obtain ECM (data not shown). Furthermore, the extent of decellularization of porcine skin treated with formic acid in different concentrations and treatment times was evaluated. Results of the histological evaluation of porcine skin before and after decellularization with H&E staining are shown in Figure 1. As shown by Figure 1A, fresh porcine skin treated with PBS as the control retained nuclei with obvious bluish-purple staining. Those porcine skins treated with 30% formic acid (Figure 1H–J) produced more obvious decellularization effects than that with 10% (Figure 1B–D) and 20% formic acid (Figure 1E–G). Moreover, porcine skin was completely decellularized after continuous treatment with 30% formic acid solution for 72 h. No presence of nuclei (bluish-purple color) or cellular remnants and a looser structure of collagen fibers were observed in decellularized porcine skin treated with 30% formic acid for 72 h (Figure 1J).
The amount of residual DNA, total collagen and GAG of porcine skin following decellularization treatments at various concentrations of formic acid for different times were measured and then compared to fresh porcine skin treated with PBS. These results are listed in Table 3. The DNA content was 349.77 ± 8.33 ng/mg dry tissue weight in porcine skin treated with PBS. DNA quantification showed a rapid decrease in the DNA amount for decellularized skin treated with formic acid and 10% and 20% formic acid had limited decellularization effects on porcine skin, as the content of residual DNA was in the range of 77~93 ng/mg dry weight. Treating porcine skin with 30% formic acid in the first 48 h decreased the DNA content to 58.87 ± 0.51 ng/mg. However, porcine skin immersed in a 30% formic acid solution exhibited decreased amounts of DNA to 67.01 ± 3.75 (19.16% ± 1.07%), 58.87 ± 0.51 (16.83% ± 0.15%) and 42.95 ± 0.73 (12.28% ± 0.21%) ng/mg dry tissue weight after being treated for 24, 48 and 72 h, respectively. Higher concentrations of formic acid solutions (30%) and longer processing times (72 h) were preferred to achieve the best decellularization effect. Prolonged treatment with formic acid, on the other hand, resulted in a compromised ECM. Our studies found that the amount of DNA remaining was 42.95 ± 0.73 ng/mg in dry porcine skin treated with 30% formic acid for 72 h. This meets the criteria for acceptable amounts of residual DNA after decellularization of <50 ng DNA per mg dry weight. Amounts of >75% total collagen still remained after decellularization with various concentrations of formic acid for different time intervals and there was no significant difference compared to the PBS group. These results showed the preservation of collagen, which is one of the major ECM components required for regeneration of skin after decellularization with different treatments in this study. The GAG content of decellularized porcine skin was significantly lower than that in the PBS group, it still remained at 5.50 ± 0.16 µg/mg dry weight (36.96% ± 1.08%) in the treatment with 30% formic acid solution for 72 h. In the 72 h treatment with 30% formic acid, complete decellularization with no presence of nuclei of cellular remnants was observed and the structural pattern of collagen fibers still remained. Although a significant loss of GAG was observed, about 37% of GAG was still retained. Therefore, 30% formic acid treatment for 72 h effectively decellularized porcine skin while retaining the greatest proportion of the ECM. The mechanism of action of formic acid on decellularization is likely due to its high permeability through porcine skin to cause swelling and DNA hydrolysis [32]. The present decellularization method of porcine skin with 30% formic acid treatment for 72 h was easy and efficient without surfactant treatment required, enabling a cost-effective and reproducible process compared to other decellularization procedures previously reported [33,34]. Further, under such a harsh condition at 30% formic acid treated for 72 h, it was expectable that bacteria and virus contamination in the porcine skin should be completely eliminated making aECM a safer biomaterial for preparation of hydrogel dressings.

3.2. Preparation and Characterization of aECM Hydrogels

Acellular ECM (aECM) obtained from porcine skin treated with 30% formic acid for 72 h was utilized to prepare aECM hydrogel. It was subjected to digest with pepsin in an acidic solution followed by neutralizing to pH value of 7 and increasing temperature to 37 °C for hydrogel formation. Effects of different concentrations of aECM digested with pepsin at 1 mg/mL concentration in different acidic solution (0.1 N HCl, GA and PCA) on the sol-gel status of hydrogels at 25 and 37 °C are shown in Table 1. At both 25 and 37 °C, formulations of aECMHCl,10, aECMGA,10 and aECMPCA,10 were observed to be in solution form, whereas that for aECMHCl,50, aECMGA,50 and aECMPCA,50 were in gel form. Favorably, formulations of aECMHCl,25, aECMGA,25 and aECMPCA,25 were observed to be in sol form at 25 °C, then transformed into a gel or glutinous form at 37 °C. This indicated that a concentration of at least 25 mg/mL of aECM was needed in order to assembly pepsin-soluble ECM fibers into 3-dimentional hydrogel structure after neutralization to a pH value of 7 and increasing temperature to 37 °C. Further, the digestion efficiency of pepsin seems to be more appropriate in 0.1 N HCl than in GA or PCA solution.
Rheological behaviors of aECMHCl,25, aECMGA,25 and aECMPCA,25 hydrogels were further evaluated at 25 and 37 °C and results are shown in Figure 2. Rheological profiles for aECMHCl,25, aECMGA,25 and aECMPCA,25 hydrogels (Figure 2A) showed to be in a sol form at 25 °C as indicated by G″ (viscous modulus) > G′ (elastic modulus), while they all transformed into a gel form at 37 °C as indicated by G′ > G″ (Figure 2B). The length of the linear viscoelastic region (LVR) of hydrogels determines the hydrogel structural stability that is a measure of hydrogel resistance to strain force. Those hydrogels with a longer length of LVR should possess a higher hydrogel strength which is only able to be destructed at a higher strain force, indicating that hydrogels could be retained firmly on the wound site. As shown by Figure 2B, the order of LVRs was as followed—aECMHCl,25 > aECMGA,25 >> aECMPCA,25. These results demonstrated that aECMHCl,25 hydrogel was optimal with a sol form at 25 °C for easier application on the wound area and transforming into a gel form at 37 °C with a gel strength higher enough for firmly retaining. Pepsin-soluble collagen (PSC) hydrogel with similar rheological behaviors has been reported by Ge et al. [15]. But it did not demonstrate that there exists a sol-gel transition characteristic at 37 °C for PSC hydrogel.
In the SEM morphological examination as shown in Figure 3, the surfaces of aECMHCl,25, aECMGA,25 and aECMPCA,25 all showed similar flaky structures (Figure 3A). Meanwhile, they all showed highly porous structures on cross-section but aECMHCl,25 possessed larger pore sizes compared to the others (Figure 3B). Figure 4 shows the SDS-PAGE electrophoretic patterns of the porcine type I collagen standard, aECMHCl,25, aECMGA,25 and aECMPCA,25. All three hydrogels of aECMHCl,25, aECMGA,25 and aECMPCA,25 displayed similar α1, α2, β and γ four bands as the collagen standard and the content of α1 was about twice that of α2, which was consistent with the molecular composition of type I collagen (α1)2α2. This seems to reveal that the structural patterns of collagen fibers still remained in the aECMHCl,25, aECMGA,25 and aECMPCA,25 samples. Overall aECMHCl,25 hydrogel was confirmed to be optimal for utilization as wound dressing with minimal loss of extracellular matrix and less modification of collagen fibers.

3.3. In Vitro Cell Viability Test

Five kinds of hydrogel dressings including HEC, CS, SC, HA and aECMHCl,25 and three kinds of composite hydrogel including aECMHCl,25/SC, HA/SC and CS/SC were selected to conduct regenerative healing studies on diabetic wounds. In vitro studies of cell viability first examined for these hydrogel dressings. After 72 h of culture, results of cell viability of WS-1 human fibroblasts with different concentrations of these hydrogel dressings are shown in Figure 5. Results showed that no hydrogel dressings possessed any toxicity at all concentrations examined (WS-1 cell viability >80%). Moreover aECMHCl,25, HA and aECMHCl,25/SC at higher concentrations (>0.05%) caused statistically significant proliferation of WS-1 cells compared to two control groups of H2O and HEC (p ≤ 0.05). It reveals that the enhancement of proliferation of WS-1 human fibroblasts by aECMHCl,25 and aECMHCl,25/SC is conformed to that as reported previously [27,35]. Promotion of fibroblast proliferation by HA hydrogel is consistent with that reported by Ciccone et al. [36]. It further confirmed that these three hydrogel dressings were very suitable for diabetic wound application.

3.4. In Vivo Wound-Healing Studies

An in vivo study of wound healing was conducted on a diabetic wound model of rats with streptozocin-induced diabetes. Photo images of wounds treated with the above-described eight types of hydrogel dressings are depicted in Figure 6A and quantitative measurements of the wound area are shown in Figure 6B. The wound lesions had completely healed after 16 days of covering with any of the wound dressings. A thin epithelial layer completely sealing the wounds was clearly visible in wounds for the aECMHCl,25, SC, aECMHCl,25/SC and HA/SC groups on day 14. A rapid drop in the remaining wound area on days 8 to 12 was observed. A significantly smaller remaining wound area was observed in the aECMHCl,25, SC, aECMHCl,25/SC and HA/SC groups compared to the HEC group after day 10 (p < 0.05) and wound lesions had completely sealed by day 14.
Histological examination of the entire wound healing process for all hydrogel dressings was performed and compared to normal skin on days 8 and 14 (Figure 7). The histological evaluation with H&E staining showed that all groups still presented wounded skin on day 8 and they showed a purple stain in the wounded areas within the green dashed lines. Newly grown tissue around the wound was observed with all dressings. The wound was in the last stage of inflammation (Figure 7A top). On day 14, the wound had closed and no inflammation was evident (Figure 7B top). A moderate number of fibroblasts occupied the dermis, which was considered remodeling in all groups. However, wounds treated with aECMHCl,25, aECMHCl,25/SC and HA/SC had healed as functional tissue with generation of hair follicles and sweat glands and exhibited complete skin regeneration. To further evaluate the wound-healing response, MT stain was used to examine the deposition of collagen in the wounds. On day 8, all groups had less collagen production with loose of structure indicating the early stage of remodeling as shown in areas within the black dashed lines (Figure 7A middle). The collagen had grown messily with no regular arrangement. Results showed that inflammation was still undergoing and the dermis demonstrated incomplete remodeling on day 8. In the aECMHCl,25, aECMHCl,25/SC and HA/SC groups, collagen had completely occupied the dermis with a uniform distribution of collagen fibers by day 14 and thus they had the most complete remodeling outcomes. Favorably, the aECMHCl,25/SC group demonstrated to have similar histologic images as that for the normal skin with a short wound-healing duration (Figure 7B middle). CD31 staining was used to evaluate vascularization in each experimental group on days 8 and 14 and results are also shown in Figure 7. As can be seen, large numbers of micro-blood vessels (red arrow) were observed in the aECMHCl,25/SC group compared to the other groups on day 8 and the wounded tissue had greater blood flow to provide sufficient oxygen and nutrition to the tissues (Figure 7A bottom). This indicated that wounds treated with aECMHCl,25/SC had proceeded to the remodeling phase by facilitating neovascularization to accelerate wound healing on day 8. However, the other groups had begun to exhibit greater vascularization only by day 14 with delayed wound healing while the aECMHCl,25/SC group exhibited the least vascularization and had full wound healing by day 14 (Figure 7B bottom). Overall, wound healing treated with various dressings was scored on the basis of scarring and H&E, MT and CD31 staining on day 14 and results were shown in Table 4. The degree of wound healing was graded from 1 to 5 depending on the extent of remodeling and the total score of normal skin was 20. It was observed for wounds treated with aECMHCl,25/SC after 14 days that the degree of remodeling in all items including scarring and H&E, MT and CD31 staining was graded as the highest among these hydrogel dressings examined. All of the above results showed that aECMHCl,25/SC had the potential to promote diabetic wound healing.
The mechanism of accelerating wound healing by the ECMHCl,25/SC hydrogels is rapid re-epithelialization and normal ECM deposition due to enhanced cellular movements in the moist microenvironment. Many studies also showed that ECM hydrogels promote cell infiltration, particularly by macrophages and progenitor cells, neovascularization and positive functional remodeling [20]. Further, aECMHCl,25/SC hydrogels accelerated wound healing to a greater extent than that for each of individual hydrogel dressings (aECMHCl,25 and SC). It indicated that there exists a potential of synergistic promotion of diabetic wound healing. The underlying mechanism responsible for that might be attributed that SC was able to promote wound healing as a result of its chemotactic effect on inflammatory cells, in turn, facilitating subsequent angiogenesis, granulation tissue formation and more-rapid new tissue formation, leading to faster wound healing [26,32]. Combination therapies with a composite hydrogel composed of aECMHCl,25 and SC hydrogel may improve the therapeutic effects of aECM hydrogels in diabetic wounds. A diabetic wound covered by an aECMHCl,25/SC hydrogel had completely healed by 14 days in the current study, whereas Hung et al. reported that skin wounds covered with an SC membrane needed 21 days [35]. It might be attributed to synergistical promotion of wound healing with a composite hydrogel. Furthermore, in comparison to SC membrane, aECMHCl,25/SC hydrogels are designed to hydrate wounds, thereby providing an ideal environment for wound healing. With their high moisture content (>90% water), they help prevent bacteria and oxygen from reaching the wound, providing a barrier against infection.
Finally, the rheological behaviors and SEM morphological image of aECMHCl,25/SC hydrogel were examined and results exhibited in Figure 8. Results reconfirmed that aECMHCl,25/SC was still the same as aECMHCl,25 in sol form at 25 °C for easier application on the wound area and was able to transform into a gel form at 37 °C with a gel strength still higher enough for firmly retaining (Figure 8A,B). Further, this composite hydrogel dressing of aECMHCl,25/SC was observed to be non-adhesive to the wound and thus can be easily removed without causing any trauma or pain. Accordingly, aECMHCl,25/SC hydrogels can potentially be utilized for accelerating diabetic wound repair and skin regeneration with all key requirements of a material that facilitates the healing process of the wound.
In comparison with wound healing effects of paste type of acellular dermal matrix subcutaneous injection reported by Lee et al. [37], it was only able to achieve 40% change in wound size for 14-day treatment of full-thickness skin defect indicating that aECMHCl,25/SC as a hydrogel form might be more beneficial to diabetic wound healing than that in paste type. However, Jeon and Kim reported that CGPaste (a paste type of acellular dermal matrix) was an effective option for coverage of small and deep chronic wounds (the mean wound area was 453.57 mm2 and the depth was 10.71 mm) by demonstrating that the wound healing occurred in five of the seven patients (71.43%) with the mean duration of complete healing being 2.4 weeks, which was similar to that for aECMHCl,25/SC as a hydrogel form [19]. Huang et al. [38] reported that after 21 days of wound healing, 80% and 84% of the wound area had re-epithelialized for symmetric Trp-rich peptides (PSI)-loaded poly (ethylene glycol) diacrylate (PEGDA)/chitosan (CS) hydrogel and PSI-plasmid Ang-1 (pANG)-loaded PEGDA/thiolated chitosan (TCS) hydrogel group, whereas only 60% and 70% of the wound area had healed for the control and PEGDA group in the meantime demonstrating that aECMHCl,25/SC as a hydrogel form illustrates better wound healing promotion efficacy as well. Lee et al. [39] reported that after applying a paste formulation of acellular dermal matrix (ADM) to the Diabetic foot ulcers (DFUs) resulted in the mean times to heal (within 60 days) of 13.54 ± 9.18 days and 21.5 ± 11.98 days, respectively, for the treatment group and the control group showing that the paste formulation of ADM equivalently provides a matrix for tissue ingrowth and promotes the healing of diabetic wound healing to that for aECMHCl,25/SC as a hydrogel form. Further, Griffin et al. [40] reported that the median time to 75% to 100% granulation being 42 days for the oxidized regenerated cellulose (ORC)/collagen/silver-ORC dressing group versus 60 days for the bovine collagen extracellular matrix (ECM), concluding that aECMHCl,25/SC as a hydrogel form might be expectable to be more favorable to diabetic wound healing.

4. Conclusions

In conclusion, a simple and effective decellularization method by treating porcine skin with 30% formic acid for 72 h was successfully developed to obtain aECM with retaining >75% collagen and ~37% GAG with the presence of the nuclei of cellular remnants to an extent of below minimal acceptable amount. The pepsin-soluble aECMHCl,25 hydrogel could be fabricated at as a minimum of 25 mg/mL concentration of so-obtained aECM digesting with 1 mg/mL of pepsin in 0.1 N HCl. aECMHCl,25 hydrogel exhibited a porous morphology with no toxicity as a biomaterial with optimal characteristics for promoting wound healing. Furthermore, a composite hydrogel consisting of aECMHCl,25 and SC (aECMHCl,25/SC) showed to synergistically accelerate wound healing and provided the healed wound with functional tissues in diabetic wound-healing studies. Ultimately, the same decellularization method to obtain aECM and the fabrication procedure of aECM hydrogel potentially play as a technical platform, on which aECM hydrogels could be created from numerous tissue sources in almost every organ system. A composite hydrogel combined with sacchachitin can then be applied to facilitate functional and constructive tissue remodeling in a variety of clinical applications in the future.

Author Contributions

Experimental investigation and analysis, C.-M.H. and Y.-H.C.; funding acquisition, W.W.; supervision and writing—original draft preparation, P.-S.W. and Y.-H.L.; writing—review and editing, H.-O.H. and M.-T.S. All authors have read and agreed to the published version of the manuscript.

Funding

This research was partially funded by the Ministry of Science and Technology, grant number MOST 107-2320-B-038-032 and Taipei Medical University (TMU106-AE1-B23).

Conflicts of Interest

The authors declare no conflict of interest. The funder had no role in the design of the study, in the collection, analyses or interpretation of data, in the writing of the manuscript or in the decision to publish the results.

References

  1. Schultz, G.S.; Ladwig, G.; Wysocki, A. Extracellular matrix: Review of its roles in acute and chronic wounds. World Wide Wounds 2005, 2005, 1–18. [Google Scholar]
  2. Bonnans, C.; Chou, J.; Werb, Z. Remodelling the extracellular matrix in development and disease. Nat. Rev. Mol. Cell Biol. 2014, 15, 786–801. [Google Scholar] [CrossRef] [PubMed]
  3. Yi, S.; Ding, F.; Gong, L.; Gu, X. Extracellular matrix scaffolds for tissue engineering and regenerative medicine. Curr. Stem Cell Res. Ther. 2017, 12, 233–246. [Google Scholar] [CrossRef] [PubMed]
  4. Kim, B.S.; Kim, H.; Gao, G.; Jang, J.; Cho, D.W. Decellularized extracellular matrix: A step towards the next generation source for bioink manufacturing. Biofabrication 2017, 9, 034104. [Google Scholar] [CrossRef]
  5. Gilbert, T.W.; Sellaro, T.L.; Badylak, S.F. Decellularization of tissue and organs. Biomaterials 2006, 27, 3657–3683. [Google Scholar] [CrossRef] [PubMed]
  6. Crapo, P.M.; Gilbert, T.W.; Badylak, S.F. An overview of tissue and whole organ decellularization process. Biomaterials 2011, 32, 3233–3243. [Google Scholar]
  7. Keane, T.J.; Swinehart, I.T.; Badylak, S.F. Methods of tissue decellularization used for preparation of biologic scaffolds and in vivo relevance. Methods 2015, 84, 25–34. [Google Scholar] [CrossRef] [Green Version]
  8. Sullivan, D.C.; Mirmalek, S.H.; Deegan, D.B.; Baptista, P.M.; Aboushwareb, T.; Atala, A.; Yoo, J.J. Decellularization methods of porcine kidneys for whole organ engineering using a high-throughput system. Biomaterials 2012, 33, 7756–7764. [Google Scholar] [CrossRef]
  9. Oliver, R.F.; Grant, R.A.; Kent, C.M. The fate of cutaneously and subcutaneously implanted trypsin purified dermal collagen in the pig. Br. J. Exp. Pathol. 1972, 53, 540–549. [Google Scholar]
  10. Prasertsung, I.; Kanokpanont, S.; Bunaprasert, T.; Thanakit, V.; Darmrongsakkul, S. Development of acellular dermis from porcine skin using periodic pressurized technique. J. Biomed. Mat. Res. Part B Appl. Biomater. 2008, 85, 210–219. [Google Scholar] [CrossRef]
  11. Arenas-Herrera, J.; Ko, I.; Atala, A.; Yoo, J. Decellularization for whole organ bioengineering. Biomed. Mater. 2013, 8, 014016. [Google Scholar] [CrossRef] [PubMed]
  12. Chen, Y.C.; Chen, R.N.; Jhan, H.J.; Liu, D.Z.; Ho, H.O.; Mao, Y.; Kohn, J.; Sheu, M.T. Development and characterization of acellular extracellular matrix scaffolds from porcine menisci for use in cartilage tissue engineering. Tissue Eng. Part C Methods 2015, 21, 971–986. [Google Scholar] [CrossRef] [PubMed]
  13. Negishi, J.; Funamoto, S.; Kimura, T.; Nam, K.; Higami, T.; Kishida, A. Effect of treatment temperature on collagen structures of the decellularized carotid artery using high hydrostatic pressure. J. Artif. Organs 2011, 14, 223–231. [Google Scholar] [CrossRef] [PubMed]
  14. Pati, F.; Jang, J.; Ha, D.H.; Kim, S.W.; Rhie, J.W.; Shim, J.H.; Kim, D.H.; Cho, D.W. Printing three-dimensional tissue and analogues with decellularized extracellular matrix bioink. Nat. Commun. 2014, 5, 3935. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  15. Ge, B.; Wang, H.; Li, J.; Liu, H.; Yin, Y.; Zhang, N.; Qin, S. Comprehensive Assessment of Nile Tilapia Skin (Oreochromis niloticus) Collagen Hydrogels for Wound Dressings. Mar. Drugs 2020, 18, 178. [Google Scholar] [CrossRef] [Green Version]
  16. Puertas-Bartolomé, M.; Benito-Garzón, L.; Fung, S.; Kohn, J.; Vázquez-Lasa, B.; Román, S.J. Bioadhesive functional hydrogels: Controlled release of catechol species T with antioxidant and antiinflammatory behavior. Mater. Sci. Eng. C 2019, 105, 110040. [Google Scholar] [CrossRef]
  17. Amato, A.; Migneco, L.M.; Martinelli, A.; Pietrelli, L.; Piozzi, A.; Francolini, I. Antimicrobial activity of catechol functionalized-chitosan versus Staphylococcus epidermidis. Carbohydr. Polym. 2018, 179, 273–281. [Google Scholar] [CrossRef] [PubMed]
  18. Mora-Boza, A.; Puertas-Bartolomé, M.; Vázquez-Lasa, B.; San Román, J.; Pérez-Caballer, A.; Olmeda-Lozano, M. Contribution of Bioactive Hyaluronic Acid and Gelatin to Regenerative Medicine, Methodologies of Gels Preparation and Advanced Applications. Eur. Polym. J. 2017, 95, 11–26. [Google Scholar] [CrossRef] [Green Version]
  19. Jeon, M.; Kim, S.Y. Application of a paste-type acellular dermal matrix for coverage of chronic ulcerative wounds. Arch. Plast. Surg. 2018, 45, 564–571. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  20. Spang, M.T.; Christman, K.L. Extracellular matrix hydrogel therapies: In vivo applications and development. Acta Biomater. 2018, 68, 1–14. [Google Scholar] [CrossRef]
  21. Saldin, L.T.; Cramer, M.C.; Velankar, S.S.; White, L.J.; Badylak, S.F. Extracellular matrix hydrogels from decellularized tissues: Structure and function. Acta Biomater. 2017, 49, 1–15. [Google Scholar] [CrossRef] [Green Version]
  22. Voytik-Harbin, S.L.; Brightman, A.O. Small intestinal submucosa: A tissue derived extracellular matrix that promotes tissue-specific growth and differentiation of cells in vitro. Tissue Eng. 1998, 4, 157–174. [Google Scholar] [CrossRef]
  23. Freytes, D.O.; Martin, J.; Velankar, S.S.; Lee, A.S.; Badylak, S.F. Preparation and rheological characterization of a gel form of the porcine urinary bladder matrix. Biomaterials 2008, 29, 1630–1637. [Google Scholar] [CrossRef] [PubMed]
  24. Agrawal, V.; Kelly, J.; Tottey, S.; Daly, K.A.; Johnson, S.A.; Siu, B.F.; Reing, J.; Badylak, S.F. An isolated cryptic peptide influences osteogenesis and bone remodeling in an adult mammalian model of digit amputation. Tissue Eng. Part A 2011, 17, 3033–3044. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  25. Parkinson, J.; Kadler, K.E.; Brass, A. Simple physical model of collagen fibrillogenesis based on diffusion limited aggregation. J. Mol. Biol. 1995, 247, 823–831. [Google Scholar] [CrossRef] [Green Version]
  26. Guo, X.; Mu, D.; Gao, F. Efficacy and safety of acellular dermal matrix in diabetic foot ulcer treatment: A systematic review and meta-analysis. Int. J. Surg. 2017, 40, 1–7. [Google Scholar] [CrossRef] [PubMed]
  27. Chao, F.C.; Wu, M.H.; Chen, L.C.; Lin, H.L.; Liu, D.Z.; Ho, H.O.; Sheu, M.T. Preparation and characterization of chemically TEMPO-oxidized and mechanically disintegrated sacchachitin nanofibers (SCNF) for enhanced diabetic wound healing. Carbohydr. Polym. 2020, 229, 115507. [Google Scholar] [CrossRef]
  28. Chen, R.N.; Lee, L.W.; Chen, L.C.; Ho, H.O.; Lui, S.C.; Sheu, M.T.; Su, C.H. Wound-healing effect of micronized sacchachitin (mSC) nanogel on corneal epithelium. Int. J. Nanomed. 2012, 7, 4697–4706. [Google Scholar]
  29. Ho, H.O.; Lin, L.H.; Sheu, M.T. Characterization of collagen isolation and application of collagen gel as a drug carrier. J. Control. Release 1997, 44, 103–112. [Google Scholar] [CrossRef]
  30. Jhan, H.J.; Liu, J.J.; Chen, Y.C.; Liu, D.Z.; Sheu, M.T.; Ho, H.O. Novel injectable thermosensitive hydrogels for delivering hyaluronic acid-doxorubicin nanocomplexes to locally treat tumors. Nanomed. UK 2014, 10, 1263–1274. [Google Scholar] [CrossRef]
  31. Masiello, P.; Broca, C.; Gross, R.; Roye, M.; Manteghetti, M.; Hillaire-Buys, D.; Novelli, M.; Ribes, G. Experimental NIDDM: Development of a new model in adult rats administered streptozotocin and nicotinamide. Diabetes 1998, 47, 224–229. [Google Scholar] [CrossRef]
  32. Lin, Y.C.; Tan, F.J.; Marra, K.G.; Jan, S.S.; Liu, D.C. Synthesis and characterization of collagen/hyaluronan/chitosan composite sponges for potential biomedical applications. Acta Biomater. 2009, 5, 2591–2600. [Google Scholar] [CrossRef] [PubMed]
  33. Khosravimelal, S.; Momeni, M.; Gholipur, M.; Kundu, S.C.; Gholipourmalekabadi, M. Protocols for decellularization of human amniotic membrane. Methods Cell Biol. 2020, 157, 37–47. [Google Scholar] [PubMed]
  34. Li, J.; Wang, M.C.; Qiao, Y.Y.; Tian, Y.Y.; Liu, J.H.; Qin, S.; Wu, W.H. Extraction and characterization of type I collagen from skin of tilapia (Oreochromis niloticus) and its potential application in biomedical scaffold material for tissue engineering. Process. Biochem. 2018, 74, 156–163. [Google Scholar] [CrossRef]
  35. Hung, W.S.; Fang, C.L.; Su, C.H.; Lai, W.F.T.; Chang, Y.C.; Tsai, Y.H. Cytotoxicity and immunogenicity of sacchachitin and its mechanism of action on skin wound healing. J. Biomed. Mater. Res. 2001, 56, 93–100. [Google Scholar] [CrossRef]
  36. Ciccone, V.; Zazzetta, M.; Morbidelli, L. Comparison of the effect of two hyaluronic acid preparations on fibroblast and endothelial cell functions related to angiogenesis. Cells 2019, 8, 1479. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  37. Lee, J.H.; Kim, J.W.; Lee, J.H.; Chung, K.J.; Kim, T.G.; Kim, Y.H.; Kim, K.J. Wound healing effects of paste type acellular dermal matrix subcutaneous injection. Arch. Plast. Surg. 2018, 45, 504–511. [Google Scholar] [CrossRef] [Green Version]
  38. Huang, L.; Zhu, Z.; Wu, D.W.; Gan, W.D.; Zhu, S.S.; Li, W.Q.; Tian, J.H.; Li, L.H.; Zhou, C.R.; Lu, L. Antibacterial poly(ethylene glycol) diacrylate/chitosan hydrogels enhance mechanical adhesiveness and promote skin regeneration. Carbohydr. Polym. 2019, 225, 115110. [Google Scholar] [CrossRef]
  39. Lee, M.; Jun, D.; Choi, H.; Kim, J.; Shin, D. Clinical Efficacy of Acellular Dermal Matrix Paste in Treating Diabetic Foot Ulcers. Wounds 2020, 1, 50–56. [Google Scholar]
  40. Griffin, L.; Carter, M.J.; D’Agostino, R., Jr.; D’Agostino McGowan, L. Comparative Effectiveness of Two Collagen-containing Dressings: Oxidized Regenerated Cellulose (ORC)/Collagen/Silver-ORC Dressing Versus Ovine Collagen Extracellular Matrix. Wounds 2019, 31, E73–E76. [Google Scholar]
Figure 1. Histological evaluation of porcine skin before (control, A) and after decellularization treated with different concentrations of formic acid (FA) (10%, B, C, D; 20%, E, G, F; and 30%, H, I, J) for 24h, B, E, H; 48h, C, F, I; and 72h, D, G, J. Scale bar: 50 μm at 200×.
Figure 1. Histological evaluation of porcine skin before (control, A) and after decellularization treated with different concentrations of formic acid (FA) (10%, B, C, D; 20%, E, G, F; and 30%, H, I, J) for 24h, B, E, H; 48h, C, F, I; and 72h, D, G, J. Scale bar: 50 μm at 200×.
Pharmaceutics 12 00538 g001
Figure 2. Rheological analysis of aECMHCl,25, aECMGA,25 and aECMPCA,25 at 25 (A) and 37 °C (B).
Figure 2. Rheological analysis of aECMHCl,25, aECMGA,25 and aECMPCA,25 at 25 (A) and 37 °C (B).
Pharmaceutics 12 00538 g002
Figure 3. Scanning electron microscopy (SEM) images ((A) surface and (B) cross-section, scale bar: 200 µm) of aECMHCl,25, aECMGA,25 and aECMPCA,25.
Figure 3. Scanning electron microscopy (SEM) images ((A) surface and (B) cross-section, scale bar: 200 µm) of aECMHCl,25, aECMGA,25 and aECMPCA,25.
Pharmaceutics 12 00538 g003
Figure 4. Sodium dodecylsulfate-polyacrylamide gel electrophoresis (SDS-PAGE) electrophoresis patterns. (A) Marker, (B) porcine type I collagen standard, (C) aECMHCl,25 hydrogel, (D) aECMGA,25 hydrogel and (E) aECMPCA,25 hydrogel.
Figure 4. Sodium dodecylsulfate-polyacrylamide gel electrophoresis (SDS-PAGE) electrophoresis patterns. (A) Marker, (B) porcine type I collagen standard, (C) aECMHCl,25 hydrogel, (D) aECMGA,25 hydrogel and (E) aECMPCA,25 hydrogel.
Pharmaceutics 12 00538 g004
Figure 5. Cell viability (n = 3) of WS-1 human skin fibroblasts incubated with five kinds of hydrogel dressings including hydroxyethyl cellulose (HEC), sacchachitin (SC), chitosan (CS) and hyaluronic acid (HA and aECMHCl,25 and three kinds of composite hydrogel including aECMHCl,25/SC, HA/SC and CS/SC at a concentration of 0.005%, 0.01%, 0.05%, 0.1% and 0.5% for 72 h. Values are presented as the mean ± standard deviation. * p < 0.05, compared to H2O.
Figure 5. Cell viability (n = 3) of WS-1 human skin fibroblasts incubated with five kinds of hydrogel dressings including hydroxyethyl cellulose (HEC), sacchachitin (SC), chitosan (CS) and hyaluronic acid (HA and aECMHCl,25 and three kinds of composite hydrogel including aECMHCl,25/SC, HA/SC and CS/SC at a concentration of 0.005%, 0.01%, 0.05%, 0.1% and 0.5% for 72 h. Values are presented as the mean ± standard deviation. * p < 0.05, compared to H2O.
Pharmaceutics 12 00538 g005
Figure 6. Wound-healing studies (n = 4~6) in diabetic rats showing the patterns of the healing process vs. time (A) with five kinds of hydrogel dressings including HEC, CS, SC, HA and aECMHCl,25 and three kinds of composite hydrogel including aECMHCl,25/SC, HA/SC and CS/SC (C); (B) The remaining wound area vs. time profiles. Values are presented as the mean ± standard deviation. * p < 0.05, compared to H2O.
Figure 6. Wound-healing studies (n = 4~6) in diabetic rats showing the patterns of the healing process vs. time (A) with five kinds of hydrogel dressings including HEC, CS, SC, HA and aECMHCl,25 and three kinds of composite hydrogel including aECMHCl,25/SC, HA/SC and CS/SC (C); (B) The remaining wound area vs. time profiles. Values are presented as the mean ± standard deviation. * p < 0.05, compared to H2O.
Pharmaceutics 12 00538 g006
Figure 7. Histologic analysis of normal skin and wounds treated with different dressings. Top to bottom displays hematoxylin and eosin (H&E), Masson’s trichrome (MT) and cluster of differentiation 31 (CD31) immunohistochemical staining. (A) Day 8, (B) day 14. Scale bar: 500 µm at 4×.
Figure 7. Histologic analysis of normal skin and wounds treated with different dressings. Top to bottom displays hematoxylin and eosin (H&E), Masson’s trichrome (MT) and cluster of differentiation 31 (CD31) immunohistochemical staining. (A) Day 8, (B) day 14. Scale bar: 500 µm at 4×.
Pharmaceutics 12 00538 g007
Figure 8. Rheological analysis of aECMHCl,25/SC wound dressing at (A) 25 and (B) 37 °C. SEM images of aECMHCl,25/SC sponge on the surface (C) and the cross-section (D) (scale bar: 200 µm).
Figure 8. Rheological analysis of aECMHCl,25/SC wound dressing at (A) 25 and (B) 37 °C. SEM images of aECMHCl,25/SC sponge on the surface (C) and the cross-section (D) (scale bar: 200 µm).
Pharmaceutics 12 00538 g008
Table 1. Effects of different concentrations of acellular extracellular matrix (aECM) digested with pepsin in different acidic solution on the sol-gel status of hydrogels at 25 and 37 °C.
Table 1. Effects of different concentrations of acellular extracellular matrix (aECM) digested with pepsin in different acidic solution on the sol-gel status of hydrogels at 25 and 37 °C.
AcronymaECM (mg/mL)Acid25 °C37 °C
aECMHCl,10100.1 N HClSolutionSolution
aECMGA,1010GASolutionSolution
aECMPCA,1010PCASolutionSolution
aECMHCl,25250.1 N HClSolutionGel
aECMGA,2525GASolutionGlu
aECMPCA,2525PCASolutionGlu
aECMHCl,50500.1 N HClGelGel
aECMGA,5050GAGelGel
aECMPCA,5050PCAGelGel
GA, glycolic acid; PCA, 2-pyrrolidone-5-carboxylic acid; Glu, Glutinous solution.
Table 2. Formulations of hydrogel dressings.
Table 2. Formulations of hydrogel dressings.
Hydrogel DressingsFormulations
HEC300 mg HEC in 20 mL ddH2O
aECMHCl,25500 mg aECMHCl,25 in 20 mL 0.1 N HCl
SC400 mg SC in 20 mL ddH2O
HA400 mg HA in 20 mL ddH2O
CS400 mg CS in 20 mL 0.1 N glycolic acid adjusted to pH 7.0 with 2 N NaOH
aECMHCl,25/SC10 mL aECMHCl,25 + 10 mL SC
HA/SC200 mg HA in 20 mL SC
CS/SC400 mg CS in 20 mL SC
HEC, hydroxyethyl cellulose; SC, sacchachitin; HA, hyaluronic acid; CS, chitosan.
Table 3. Contents of residual DNA, total collagen and glycosaminoglycan (GAG) of porcine skin following decellularization at various concentrations of formic acid (FA) for different time points compared to fresh porcine skin treated with phosphate-buffered saline (PBS) under the same processing steps. Values are presented as the mean ± standard deviation (n = 3). (* p < 0.05 compared to fresh porcine skin treated with PBS).
Table 3. Contents of residual DNA, total collagen and glycosaminoglycan (GAG) of porcine skin following decellularization at various concentrations of formic acid (FA) for different time points compared to fresh porcine skin treated with phosphate-buffered saline (PBS) under the same processing steps. Values are presented as the mean ± standard deviation (n = 3). (* p < 0.05 compared to fresh porcine skin treated with PBS).
Treatments0 h24 h48 h72 h
Residual DNA (ng/mg dry weight)
PBS349.77 ± 8.33---
10% FA-93.43 ± 1.14 *90.89 ± 2.02 *87.16 ± 2.86 *
20% FA-87.84 ± 0.85 *87.35 ± 3.90 *77.32 ± 0.82 *
30% FA-67.01 ± 3.75 *58.87 ± 0.51 *42.95 ± 0.73 *
Total collagen (µg/mg dry weight)
PBS715.39 ± 7.34---
10% FA-647.15 ± 18.51630.45 ± 13.43625.87 ± 2.38
20% FA-610.25 ± 2.13583.85 ± 3.90566.52 ± 7.34
30% FA-574.69 ± 7.46567.24 ± 7.97556.01 ± 5.94
Glycosaminoglycan (µg/mg dry weight)
PBS14.88 ± 1.21---
10% FA-10.61 ± 0.32 *8.97 ± 0.40 *9.59 ± 0.32 *
20% FA-9.19 ± 0.08 *7.79 ± 0.08 *6.52 ± 0.32 *
30% FA-7.09 ± 0.64 *6.86 ± 0.80 *5.50 ± 0.16 *
Table 4. Overall assessment for in vivo wound healing studies on day 14.
Table 4. Overall assessment for in vivo wound healing studies on day 14.
Wound DressingsScarringH&EMTCD31Sum of Grading Score
Normal skin555520
HEC11136
ECMHCl433414
SC41139
HA31138
CS11136
ECMHCl+SC445417
HA+SC423312
CS+SC21137
Note: The degree of wound healing was graded from 1 to 5 depending on the extent of remodeling: 1 = minimal (1%~20%); 2 = slight (21%~40%); 3 = moderate (41%~60%); 4 = moderately high (61%~80%); 5 = high (81%~100%). H&E, hematoxylin and eosin; MT, Masson’s trichrome; CD31, cluster of differentiation 31.

Share and Cite

MDPI and ACS Style

Hsieh, C.-M.; Wang, W.; Chen, Y.-H.; Wei, P.-S.; Liu, Y.-H.; Sheu, M.-T.; Ho, H.-O. A Novel Composite Hydrogel Composed of Formic Acid-Decellularized Pepsin-Soluble Extracellular Matrix Hydrogel and Sacchachitin Hydrogel as Wound Dressing to Synergistically Accelerate Diabetic Wound Healing. Pharmaceutics 2020, 12, 538. https://0-doi-org.brum.beds.ac.uk/10.3390/pharmaceutics12060538

AMA Style

Hsieh C-M, Wang W, Chen Y-H, Wei P-S, Liu Y-H, Sheu M-T, Ho H-O. A Novel Composite Hydrogel Composed of Formic Acid-Decellularized Pepsin-Soluble Extracellular Matrix Hydrogel and Sacchachitin Hydrogel as Wound Dressing to Synergistically Accelerate Diabetic Wound Healing. Pharmaceutics. 2020; 12(6):538. https://0-doi-org.brum.beds.ac.uk/10.3390/pharmaceutics12060538

Chicago/Turabian Style

Hsieh, Chien-Ming, Weu Wang, Ying-Hsuan Chen, Pu-Sheng Wei, Yu-Hsuan Liu, Ming-Thau Sheu, and Hsiu-O Ho. 2020. "A Novel Composite Hydrogel Composed of Formic Acid-Decellularized Pepsin-Soluble Extracellular Matrix Hydrogel and Sacchachitin Hydrogel as Wound Dressing to Synergistically Accelerate Diabetic Wound Healing" Pharmaceutics 12, no. 6: 538. https://0-doi-org.brum.beds.ac.uk/10.3390/pharmaceutics12060538

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop