Next Article in Journal
Thermal Positioning Error Modeling of Servo Axis Based on Empirical Modeling Method
Next Article in Special Issue
Cutting Force Prediction Models by FEA and RSM When Machining X56 Steel with Single Diamond Grit
Previous Article in Journal
Surface-Potential-Based Compact Modeling of p-GaN Gate HEMTs
Previous Article in Special Issue
Effect of Strain Rate on the Deformation Characteristic of AlN Ceramics under Scratching
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Research on Precision Blanking Process Design of Micro Gear Based on Piezoelectric Actuator

School of Mechanical and Electrical Engineering, Suqian College, Suqian 223800, China
*
Author to whom correspondence should be addressed.
Submission received: 2 February 2021 / Revised: 10 February 2021 / Accepted: 13 February 2021 / Published: 15 February 2021
(This article belongs to the Special Issue Micro and Nano Machining Processes)

Abstract

:
In order to process micro scale parts more conveniently, especially the micro parts with complex shape, a new micro blanking equipment based on piezoelectric ceramic driving is proposed in this paper. Compared with other large precision machining equipment, the equipment cost has been greatly reduced. Using displacement sensor to detect the change of output displacement and feedback control piezoelectric actuator to control the change of relevant parameters, the control precision is high. The micro gear parts with diameter less than 2 mm are obtained through the blanking experiment on the experimental equipment. From the relationship between the obtained time and the punch output force, output displacement and die adjustment, it can be seen that the designed equipment has good processing performance and can complete the blanking forming of micro parts well.

1. Introduction

The miniaturization of industrial equipment, especially medical equipment and electronic equipment, is to meet the requirements of the development of modern medical science and precision instruments, so the components of these equipment must be more miniaturized and high-precision. For these micro scale parts, different from traditional size parts, special processing methods must be used. For example, laser dynamic flexible punching process, electrical-field activated sintering, metal powder compaction in elastic dies, and micro wire electrical discharge machining are the common processing methods studied at present [1,2,3,4]. For gears of traditional size, we have various mature processing technologies, which can meet the technological requirements of various traditional equipment for gears. However, the micro gear cannot be realized by the traditional cutting technology. The thickness of the gear teeth is very thin. When the traditional technology is used for processing, the gear teeth are easily broken. At present, some mold manufacturers in the mechanical industry can obtain the pinion by wire cutting, but the size of the gear they can process cannot be too small, because once the size of the gear is less than 1–2 mm, very thin electrode wire must be competent, which will greatly increase the cost [5,6,7,8,9,10]. Maher et al. provided a method for increasing the productivity of the wire-cut electrical discharge machine [11]. Chen et al. analyzed the geometrical inaccuracy in WEDM rough corner cutting [12]. Jianwen et al. studied micro gear fabrication in laser dynamic flexible punching [13]. Horiuchi et al. put forward micro gear fabrication using optical projection lithography on copper-clad plastic substrates and electroplating of nickel [14]. Cannella, E.; Nielsen, E.K.; Stolfi, A. designed a tool system for lowering friction during the ejection of in-die sintered micro gears [15]. Garner, S.; Ruiz, E.; Strong, J.; Zavaliangos, A. studied mechanisms of crack formation in die compacted powders during unloading and ejection [16]. Akarachkin, S.A.; Ivashutenko, A.S.; Martyushev, N.V. studied activation of mass transfer processes at spark plasma sintering of zirconium dioxide [17]. Zhong et al. provided micro-stepped gear mold fabrication based on WEDM and thermal diffusion welding [18]. Álvarez et al. provided a large spiral bevel gear fabrication on universal 5-axis milling machines [19]. Yohei and Hirota studied precision stamping process of metal micro gears [20,21]. Peng-Zhi et al. studied dynamic linear modeling, identification and precise control of a walking piezo-actuated stage—ScienceDirect [22]. Wang et al. established a new hysteresis modeling and analysis feed forward control of piezoelectric actuators based on asymmetric Prandtl-Ishlinskii model [23]. Peng-Zhi et al. studied “Piezoelectric Actuated Phase Shifter Based on External Laser Interferometer: Design, Control and Experimental Validation” [24]. Bo et al. studied “5-axis double-flank CNC machining of spiral bevel gears via custom-shaped milling tools—Part I: Modeling and simulation” [25]. The equipment designed in this paper can get micro gears by means of punching, with a diameter of addendum circle less than 2 mm, and the gear is a kind of tooth with addendum and root trimming. In order to make the blanking surface of the gear more fine, when the working material becomes very thin, it is necessary to provide a very narrow gap evenly between the punch and the die along the contour of the part. Generally, according to the results of precision blanking, the gap is set to about 1% of the thickness of the workpiece.

2. Experimental Device Design

2.1. Micro Gear Parts

Figure 1 is the part drawing of the involute micro gear to be processed. The basic specification of the gear is that the reference circle diameter is 1.8 mm, the number of teeth is 12, and the module is 0.15 mm. The workpiece material is H62, the tooth thickness t is 235.5 μm, and the tooth width B is 0.5 mm. Table 1 shows the performance parameters of workpiece materials.

2.2. Structure of Experimental Device

The deformation of single-layer ceramic is limited. In this project, the piezoelectric ceramic driver is designed by stacking multi-layer piezoelectric ceramic, as shown in Figure 2. The workpiece is punched and cut under the action of external voltage. In the piezoelectric ceramic stack structure, each piece of ceramic is embedded in the electrode to form a mechanical series connection and a circuit parallel connection. The relationship between the elongation of piezoelectric ceramic stack structure and input voltage is:
Δ l = n ξ u + n m u 2 / t
where Δ l   is total elongation, n is the number of piezoelectric ceramics,   ξ is piezoelectric coefficient, u is input voltage, t is the thickness of each piezoelectric ceramic, n = 27. Figure 3 shows the open-loop voltage and displacement curve of piezoelectric ceramics.
The relevant values of die root diameter and punch tip diameter are listed in Table 2:

2.3. Calculation of Precision Blanking Process Force

The stress during precision blanking is shown in Figure 4. In the punching process, the workpiece receives the blank holder force F2, the punching force F1 and the counter pressure F3 at the same time.

2.3.1. Calculation of the Punching Force

The blanking force F1 can be calculated by Formula (2):
F 1 = f 1 l t t σ b
where f 1 is a coefficient that depends on the yield ratio σ s σ b of the material. Considering that the die gap is small and the material is in a three-dimensional compressive stress state during precision blanking, the deformation resistance is greater than that of general blanking, with f 1 = 0.9 ;
l t is the outline peripheral length;
t is the workpiece thickness;
σ b is the tensile strength of materials.
In order to get the contour length l, the involute length of one-side of gear teeth is calculated first [26], and its calculation formula is:
l i n v = 0.5 r b ( t a n 2 α a t a n 2 α b ) = 0.5 r b t a n 2 α a
where l i n v is the involute length;
r b is the radius of base circle;
α a is the pressure angle of addendum circle;
α b is the pressure angle of base circle.
The tooth thickness on different circles is calculated as Formula (4) [26,27]:
φ d = s / r 2 ( i n v α d i n v α )
where φ d is the central angle of tooth thickness on a circle with diameter d;
s is the tooth thickness of graduation circle;
r is the radius of reference circle;
α d is the pressure angle of tooth thickness on a circle with diameter d;
α d is the pressure angle of graduation circle.
The total length of contour circumference is obtained as Formula (5):
l t = 2 × z × l i n v + z × s a + ( π d b z × s b )
where z is teeth number of the gear;
s a is the tooth thickness on addendum circle;
s b is the tooth thickness on base circle;
d b is the diameter of base circle.
Comprehensive of Formulas (3)–(5), the calculation results of the total length of contour circumference are as follows:
l t 8.8228 mm
Substituting l t , t, f1 and σ b into Formula (2), the value of blanking force F1 is:
F 1 = f 1 l t t σ b = 0.9 × 8.8228 × 0.5 × 370 1469 N

2.3.2. Calculation of the Blank Holder Force

The calculation method of blank holder force can be obtained from the empirical formula of Reference [27]:
F 2 = f 2 l t 2 h σ b = 1.5 × 8.8228 × 2 × 0.3 × 370 2938 N
where h is v-shaped tooth height of blank holder.

2.3.3. Calculation of the Counter Pressure

The value of the back pressure F3 will have an impact on the dimensional accuracy, flatness, collapse angle and the quality of the shear plane of the workpiece. Increasing the back pressure appropriately will improve the above indexes, but excessive back pressure will increase the punch load. Back pressure of fine blanking process can be calculated by Formula (6) [27]:
F 3 = p A
where p is unit back pressure, generally taken at 20~70 N/mm2, with p = 55 N/mm2; A is the end area of part; the calculation formula can be obtained from Reference [26].
A = ( 0.5 s / r + i n v α ) ( r a 2 r b 2 ) ( i n v α a r a 2 i n v α b r b 2 ) + 2 r b 2 ( t a n 3 α a t a n 3 α b ) / 6
Substituting all data into Formula (7), we can obtain:
A = 0.03265 mm 2
  F 3 = 55 × 0.03265 = 1.796 N

2.3.4. Total Pressure Calculation

The total pressure required by the workpiece to finish the fine blanking process is the main basis for the design of stamping equipment. The workpiece should be blanked before fine blanking to ensure reliable blank pressing. The total pressure includes blanking force and back pressure, which can be calculated as follows:
F = F 1 + F 3 = 1469 + 1.796 = 1470.8 N

3. Simulation of Micro Gear Blanking

3.1. Simulation Model

We used Solid Edge software to build 3D model and save it in STL format. Then, we imported STL file into DEFORM software and adjusted the position of each part to form the original model as shown in Figure 5. The blank is pressed on the upper surface of the gear die by a pressing block, and the punch is placed on the top surface of the blank.
Figure 6a is the blank after the micro gear blanking simulation, whose size is consistent with the actual size and Figure 6b is the blank after the micro gear blanking on the designed micro forming equipment, whose size and actual size ratio is 3:1. From Figure 6a, the simulation blanking is very close to the desired shape, so the model can get the simulation results more accurately, and can do further research on the blanking process of the designed equipment. From Figure 6b, we can see the teeth obtained on the equipment are with tip relief and bottom relief. D. Martínez Krahmer et al.’s research on the edge quality affected fatigue or tensile strength, whose results show that some changes on surface state appeared, but the effect on tensile strength was lower than 5% [28].

3.2. Analysis of Blanking Stress

Figure 7a is the effective stress diagram of the punch in the simulation analysis of micro gear blanking. AB section is the stage of elastic deformation. At the beginning, the punch contacts with the blank and produces downward pressure. The blank is bent and deformed, and the blanking force increases approximately vertically in a short time until it reaches the yield strength of the blank. For yield deformation, such as BC section, the blanking force increases slowly and increases with the movement of the punch, reaching the yield strength at C point maximum. At this stage, the stress in the deformation zone of the blank exceeds its yield strength, the sheet metal is pressed into the die, plastic deformation occurs, and large stress occurs at the contact edge of the die, and then the stress value exceeds the shear strength, and the blank begins to crack. The blank starts to fracture in the CD section, the punch continues to move, the blanking force gradually decreases, the blank crack continues to extend until it is completely separated, the blanking process is completed, and then the blanking force decreases vertically.
Figure 7b is the effective stress diagram of the die in the simulation analysis of micro gear blanking. The blank of AB section is elastic deformation, and the blanking force increases approximately vertically in a short time until it reaches the yield strength of the blank. The blank produces yield deformation. At the beginning of BC section, the die stress transits from elastic deformation to plastic deformation step by step. At this stage, the die stress increases, and then decreases to C. At this point, the sheet metal is pressed into the die, and a large stress is generated at the contact edge of the die, and the stress value exceeds the shear strength. The blank begins to crack, the thickness of the blank joint decreases, the punch continues to move, the blanking force on the die gradually decreases, and the blank crack continues to extend and expand until it is completely separated. The blanking process ends, and then the blanking force in the DE section decreases vertically.
There are three hundred steps in the whole simulation process. The effective strain of blank is shown in Figure 8 for every 70 steps. It can be seen that the model can obtain the ideal simulation results.

4. Experiment of Micro Gear Forming

4.1. Structure of Micro Gear Forming Device

Figure 9 shows the designed micro gear forming device, which uses the principle that piezoelectric ceramics can produce output displacement with the change of input voltage, and can produce larger output force to drive the punch to achieve stamping action. The blank is pressed on the upper surface of the die by the pressing block, and the die is fixed on the worktable. A displacement sensor is set under the worktable to obtain the impact displacement and feed it back to the controller. The punch is fixed on the upper bracket, and the punch and the die are strictly aligned during installation.

4.2. Change of Micro Gear Processing Parameters

Figure 10 shows the relationship between output and time. Line 1 is the diagram of punch impact force versus time; Line 2 shows the change between punch displacement and time; Line 3 is the diagram of die adjusting displacement with time. Micro gear parts can be easily obtained by reasonable parameter setting.

4.3. Micro Gear Parts Formed by Blanking on the Device

Figure 11a shows the micro gear parts obtained, with module of 0.15 mm, number of teeth of 12 and tooth width of 0.5 mm. Figure 11b is a micrograph of the die. It can be seen from the figure that the profile of the formed gear is clear and there is no burr on the profile surface. The main reason is that during stamping, the blank of the part is fixed firmly and reliably, and the pressure stress produced by the punch is evenly distributed, the material is pressed into the die through several strokes of the punch, the surface of the part is extruded flat inside the die surface, with high dimensional accuracy and small surface roughness.

5. Discussion

A set of device for precision forming of micro parts based on piezoelectric ceramic driver is developed. (1) Through the displacement sensor detection and feedback, the position adjustment of the precision electric displacement table is realized, so as to complete the adjustment of the machining position of the parts. (2) The control system of the device is designed. By selecting the appropriate control parameters, the device can run stably and reliably. (3) The tooth profile of the micro gear is clear, and the microhardness meets the requirements of the gear, so the designed micro stamping system can form the micro parts with good quality.

Author Contributions

C.H. designed the experimental equipment, operated the experiments, analyzed the results, wrote the paper, reviewed and edited the paper. Y.S. carried out the simulation, supported the experiments. F.L. designed the micro-gear shape. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by Suqian Industrial Guidance Fund Project [H201821], Suqian 1000 Leading Talents Gathering Project and Six Talent Peak Projects in Jiangsu Province [GDZB-270].

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Liu, H.X.; Lu, M.M.; Wang, X.; Shen, Z.B.; Gu, C.X.; Gu, Y.X. Micro-punching of aluminum foil by laser dynamic flexible punching process. Int. J. Mater. Form. 2013, 8, 183–196. [Google Scholar] [CrossRef]
  2. Ni, X.L.; Yin, H.Q.; Liu, L.; Yi, S.J.; Qu, X.H. Injection molding and debinding of micro gears fabricated by micro powder injection molding. Int. J. Min. Met. Mater. 2013, 1, 82–87. [Google Scholar] [CrossRef]
  3. Zhao, J.; Qin, Y.; Huang, K.; Hijji, H. Forming of micro-components by electrical-field activated sintering. MATEC Web Conf. 2015, 21, 10001. [Google Scholar] [CrossRef] [Green Version]
  4. Noveanu, D. Researches concerning a new method for obtaining spur gears by metal powder compaction in elastic dies. Metalurgia 2013, 65, 35–39. [Google Scholar]
  5. Wang, Y.; Chen, X.; Wang, Z.; Dong, S. Fabrication of micro gear with intact tooth profile by micro wire electrical discharge machining. J. Mater. Process. Technol. 2017, 9, 002. [Google Scholar]
  6. Gupta, K.; Jain, N.K. Comparative Study of Wire-EDM and Hobbing for Manufacturing High-Quality Miniature Gears. Mater. Manuf. Process. 2014, 29, 1470–1476. [Google Scholar] [CrossRef]
  7. Habib, S.; Okada, A. Study on the movement of wire electrode during fine wire electrical discharge machining process. J. Mater. Process. Technol. 2016, 227, 147–152. [Google Scholar]
  8. Gupta, K.; Jain, N.K. Analysis and optimization of micro-geometry of miniature spur gears manufactured by wire electric discharge machining. Precis. Eng. 2014, 38, 728–737. [Google Scholar] [CrossRef]
  9. Chen, X.; Wang, Z.; Xu, J.; Wang, Y.; Li, J.; Liu, H. Sustainable production of micro gears combining micro reciprocated wire electrical discharge machining and precision forging. J. Clean. Prod. 2018, 188, 1–11. [Google Scholar] [CrossRef]
  10. Wang, Y.K.; Chen, X.; Wang, Z.L.; Dong, S.L. Fabrication of micro gear with intact tooth profile by micro wire electrical discharge machining. J. Mater. Process. Technol. 2018, 252, 137–147. [Google Scholar] [CrossRef]
  11. Maher, I.; Sarhan, A.A.; Barzani, M.M.; Hamdi, M. Increasing the productivity of the wire-cut electrical discharge machine associated with sustainable production. J. Clean. Prod. 2015, 108, 247–255. [Google Scholar] [CrossRef]
  12. Chen, Z.; Huang, Y.; Zhang, Z.; Li, H.; Ming, W.Y.; Zhang, G.J. An analysis and optimization of the geometrical inaccuracy in WEDM rough corner cutting. Int. J. Adv. Manuf. Technol. 2014, 74, 917–929. [Google Scholar] [CrossRef]
  13. Li, J.; Liu, H.; Shen, Z.; Qian, Q.; Zhang, H.; Wang, X. Formability of micro-gears fabrication in laser dynamic flexible punching. J. Mater. Process. Technol. 2016, 234, 131–142. [Google Scholar] [CrossRef]
  14. Horiuchi, T.; Furuuchi, Y.; Nakamura, R.; Hirota, K. Micro-gear fabrication using optical projection lithography on copper-clad plastic substrates and electroplating of nickel. Microelectron. Eng. 2006, 83, 1316–1320. [Google Scholar] [CrossRef]
  15. Cannella, E.; Nielsen, E.K.; Stolfi, A. Designing a tool system for lowering friction during the ejection of in-die sintered micro gears. Micromachines 2017, 8, 214. [Google Scholar]
  16. Garner, S.; Ruiz, E.; Strong, J.; Zavaliangos, A. Mechanisms of crack formation in die compacted powders during unloading and ejection: An experimental and modeling comparison between standard straight and tapered dies. Powder Technol. 2014, 264, 114–127. [Google Scholar] [CrossRef]
  17. Akarachkin, S.A.; Ivashutenko, A.S.; Martyushev, N.V. Activation of mass transfer processes at spark plasma sintering of zirconium dioxide. IOP Conf. Ser. Mater. Sci. Eng. 2016, 124, 12042. [Google Scholar] [CrossRef] [Green Version]
  18. Zhong, J.M.; Wu, X.Y.; Xu, B.; Ruan, S.C. Laminated fabrication of micro-stepped gear mold based on WEDM and thermal diffusion welding. Inter. J. Adv. Manuf. Technol. 2015, 78, 1233–1240. [Google Scholar] [CrossRef]
  19. Álvarez, A.; de López Lacalle, L.N.; Olaiz, A.; Rivero, A. Large Spiral Bevel Gears on Universal 5-axis Milling Machines: A Complete Process. Procedia Eng. 2015, 132, 397–404. [Google Scholar] [CrossRef] [Green Version]
  20. Suzuki, Y.; Shiratori, T.; Murakawa, M.; Yang, M. Precision stamping process of metal micro gears. Procedia Manuf. 2018, 15, 1445–1451. [Google Scholar]
  21. Hirota, K. Precision blanking method with negative clearance. J. Serv. Theor. Pract. 2014, 185–189. [Google Scholar]
  22. Li, P.Z.; Wang, X.D.; Zhao, L.; Zhang, D.F.; Guo, K. Dynamic linear modeling, identification and precise control of a walking piezo-actuated stage. Mech. Syst. Signal Process. 2019, 128, 141–152. [Google Scholar] [CrossRef]
  23. Wang, W.; Wang, R.; Chen, Z.; Sang, Z.; Ju, B. A new hysteresis modeling and feedforward control of piezoelectric actuators based on asymmetric Prandtl-Ishlinskii model. Sensor. Actuat. A Phys. 2020, 316, 112431. [Google Scholar] [CrossRef]
  24. Li, P.Z.; Wang, X.D.; Sui, Y.X.; Zhang, D.F.; Wang, D.F.; Dong, L.J.; Ni, M.Y. Piezoelectric actuated phase shifter based on external laser interferometer: Design, control and experimental validation. Sensors 2017, 17, 838. [Google Scholar] [CrossRef] [Green Version]
  25. Bo, P.; González, H.; Calleja, A.; de Lacalle, L.N.; Bartoň, M. 5-axis double-flank CNC machining of spiral bevel gears via custom-shaped milling tools—Part I: Modeling and simulation. Precis. Eng. 2019, 62, 204–212. [Google Scholar] [CrossRef] [Green Version]
  26. Meek, D.S.; Walton, D.J. Calculation of involute substitute arc by two-point equal arc method. Modern Manuf. Eng. 1982, 10, 22–23. [Google Scholar]
  27. Yulong, L.; Kun, L. Established Formulas for Trapped-oil Area and Relief-load Area of External Spur-gear Pump. Trans. Chin. Soc. Agric. Mach. 2009, 40, 203–207. [Google Scholar]
  28. Krahmer, D.M.; Polvorosa, R.; De Lacalle, L.L.; Alonso-Pinillos, U.; Abate, G.; Riu, F. Alternatives for specimen manufacturing in tensile testing of steel plates. Exp. Tech. 2016, 40, 1555–1565. [Google Scholar] [CrossRef]
Figure 1. Part drawing of micro gear.
Figure 1. Part drawing of micro gear.
Micromachines 12 00200 g001
Figure 2. The internal structure of packaged piezoelectric ceramics. 1. Drive power line; 2. Fixed sea; 3. Package shell; 4. Laminated piezoelectric ceramics; 5. Disk spring; 6. Output shaft; 7. Linear bearing; 8. Locking cover.
Figure 2. The internal structure of packaged piezoelectric ceramics. 1. Drive power line; 2. Fixed sea; 3. Package shell; 4. Laminated piezoelectric ceramics; 5. Disk spring; 6. Output shaft; 7. Linear bearing; 8. Locking cover.
Micromachines 12 00200 g002
Figure 3. The open-loop voltage and displacement curve of piezoelectric ceramics. Line 1: Relationship between rising input voltage and measured output displacement; Line 2: Relationship between down input voltage and measured output displacement.
Figure 3. The open-loop voltage and displacement curve of piezoelectric ceramics. Line 1: Relationship between rising input voltage and measured output displacement; Line 2: Relationship between down input voltage and measured output displacement.
Micromachines 12 00200 g003
Figure 4. The stress during precision blanking. 1. Compaction block; 2. Workpiece; 3. Workbench.
Figure 4. The stress during precision blanking. 1. Compaction block; 2. Workpiece; 3. Workbench.
Micromachines 12 00200 g004
Figure 5. The simulation model of micro gear blanking processing. 1. Punch; 2. Workpiece; 3. Die; 4. Press plate; 5. Screw.
Figure 5. The simulation model of micro gear blanking processing. 1. Punch; 2. Workpiece; 3. Die; 4. Press plate; 5. Screw.
Micromachines 12 00200 g005
Figure 6. (a) The blank after the micro gear blanking simulation; (b) The blank after the micro gear blanking on the designed micro forming equipment.
Figure 6. (a) The blank after the micro gear blanking simulation; (b) The blank after the micro gear blanking on the designed micro forming equipment.
Micromachines 12 00200 g006
Figure 7. (a) The effective stress diagram of the punch in the simulation analysis of micro gear blanking; (b) The effective stress diagram of the die in the simulation analysis of micro gear blanking.
Figure 7. (a) The effective stress diagram of the punch in the simulation analysis of micro gear blanking; (b) The effective stress diagram of the die in the simulation analysis of micro gear blanking.
Micromachines 12 00200 g007
Figure 8. Stress effect of billet in different simulation steps.
Figure 8. Stress effect of billet in different simulation steps.
Micromachines 12 00200 g008aMicromachines 12 00200 g008b
Figure 9. Stress effect of billet in different simulation steps.
Figure 9. Stress effect of billet in different simulation steps.
Micromachines 12 00200 g009
Figure 10. The relationship between output and time. Line 1: Diagram of punch impact force versus time; Line 2: Diagram of punch displacement versus time; Line 3: Diagram of die adjusting displacement with time.
Figure 10. The relationship between output and time. Line 1: Diagram of punch impact force versus time; Line 2: Diagram of punch displacement versus time; Line 3: Diagram of die adjusting displacement with time.
Micromachines 12 00200 g010
Figure 11. Micrograph of formed gear and die. (a) Micro gear parts formed by machining, (b) Partial screenshot of die gear teeth
Figure 11. Micrograph of formed gear and die. (a) Micro gear parts formed by machining, (b) Partial screenshot of die gear teeth
Micromachines 12 00200 g011
Table 1. Performance parameters of workpiece materials.
Table 1. Performance parameters of workpiece materials.
ItemValue
Material compositionCu 60.5%~63.5%
Tensile strength (Mpa)370
Modulus of elasticity (Gpa)100
Vickers hardness (HV)115
Coefficient of linear expansion (*106)20.6
Fatigue limit (Mpa)154
Yield strength (Mpa)120
Table 2. Main parameters of blanking device.
Table 2. Main parameters of blanking device.
ItemValue
Unilateral Gap CL (μm)5
Addendum Circle Diameter of Punch dP0 (mm)1.95
Root Circle Diameter of Die dD0 (mm)1.85
Outer Diameter of Die dD (mm)25.0
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Hu, C.; Shi, Y.; Liu, F. Research on Precision Blanking Process Design of Micro Gear Based on Piezoelectric Actuator. Micromachines 2021, 12, 200. https://0-doi-org.brum.beds.ac.uk/10.3390/mi12020200

AMA Style

Hu C, Shi Y, Liu F. Research on Precision Blanking Process Design of Micro Gear Based on Piezoelectric Actuator. Micromachines. 2021; 12(2):200. https://0-doi-org.brum.beds.ac.uk/10.3390/mi12020200

Chicago/Turabian Style

Hu, Changjun, Yunyang Shi, and Fangfang Liu. 2021. "Research on Precision Blanking Process Design of Micro Gear Based on Piezoelectric Actuator" Micromachines 12, no. 2: 200. https://0-doi-org.brum.beds.ac.uk/10.3390/mi12020200

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop