Next Article in Journal
Lauric Acid Hybridizing Fly Ash Composite for Thermal Energy Storage
Next Article in Special Issue
Property and Microstructure of Waterborne Self-Setting Geopolymer Coating: Optimization Effect of SiO2/Na2O Molar Ratio
Previous Article in Journal
The Evidence of Decisive Effect of Both Surface Microstructure and Speciation of Chalcopyrite on Attachment Behaviors of Extreme Thermoacidophile Sulfolobus metallicus
Previous Article in Special Issue
The Role of Clay Swelling and Mineral Neoformation in the Stabilization of High Plasticity Soils Treated with the Fly Ash- and Metakaolin-Based Geopolymers
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Experimental Evaluation of Efficient Si Dissolution from Perlite at Low Level Activator’s Concentration

School of Mining and Metallurgical Engineering, National Technical University of Athens, 157 80 Athens, Greece
*
Author to whom correspondence should be addressed.
Submission received: 20 March 2018 / Revised: 29 March 2018 / Accepted: 30 March 2018 / Published: 14 April 2018
(This article belongs to the Special Issue Geopolymers)

Abstract

:
This paper deals with the Si dissolution of fine perlite in alkaline solutions for the determination of the SiO2/Na2O mass ratio in the aqueous phase of geopolymer slurries. In the present work, the effect of the main synthesis parameters such as NaOH concentration and curing temperature on the setting time of the paste were studied. The obtained results showed that the inorganic polymer pastes present fast hardening at low concentrations of NaOH solutions for both 70 and 90 °C. This observation was also identified by the Si dissolution study of perlite pastes as a function of different concentrations of NaOH solutions and different solid to liquid ratios of the slurries, under a constant temperature. The optimum synthesis conditions for geopolymer pastes proved to be a low initial NaOH concentration in the alkaline phase (2–4 M NaOH), where the fast hardening of the paste was attributed to the high SiO2/Na2O mass ratio, enhancing the polycondensation phenomena and promoting the geopolymerization process.

1. Introduction

Extended research activity in the field of geopolymer synthesis over the last decade has proved that geopolymers possess excellent mechanical and physicochemical properties. According to these properties, inorganic polymers are considered ideal alternatives for many industrial applications, mainly in the construction sector. Geopolymerization is based on an exothermic heterogeneous chemical reaction between a solid aluminosilicate raw material and an alkali metal silicate solution under atmospheric conditions and temperatures up to 100 °C. The materials synthesized by this reaction present mainly an amorphous or semi-crystalline Si–O–Al and/or Si–O–Si frame. A variety of industrial solid residues or wastes such as fly ashes, metallurgical slags, and mine wastes, as well as industrial minerals such as kaolinite and feldspars [1,2,3,4,5,6,7,8,9,10], have been used for the synthesis of geopolymers. The produced materials exhibit remarkable properties, depending on the mix design and on the applications for which they are intended, such as high surface hardness, high mechanical strength, fire and chemical resistance, thermal stability, low density, and micro or nano porosity [11,12,13,14,15,16,17,18].
However, perlite has not been extensively studied as a potential aluminosilicate source for the synthesis of inorganic polymers through geopolymerization technology. The main reason for this is that perlite has been considered as an inefficient raw material for geopolymerization, resulting in final materials with a lack of mechanical properties [19]. Perlite deposits are normally exploited with low-cost open pit mining methods followed by in situ milling and screening. Greece and Turkey are the world’s leading perlite producers, with an annual production for the year 2017 of 700,000 t and 1,100,000 t per country [20], while in Europe the annual production of perlite was estimated to be about 1,935,000 t for 2017 [20].
This paper deals with the investigation of perlite geopolymer paste’s setting time, as a function of different NaOH solution concentrations, at two temperatures. The results were evaluated by the determination of the SiO2/Na2O mass ratio, which corresponds to the geopolymer pulps after two series of Si dissolution tests from perlite in an alkaline activator. In the first series, Si dissolution of perlite in NaOH solutions of different concentrations and temperatures was determined at a constant solid to liquid ratio. The second experimental series included Si dissolution tests of the perlite pulps as a function of different alkaline activator concentrations at different solid to liquid ratios for a constant temperature. Finally, the SiO2/Na2O mass ratio of the examined pulps was determined, indicating (after an extrapolation process) a possible SiO2/Na2O value for the real solid to liquid ratio of the geopolymer paste.

2. Materials and Methods

2.1. Materials

The raw materials used for the synthesis of geopolymer slurries consist of sodium hydroxide and expanded perlite wastes from the milling plant of Imerys on Milos Island, Greece. The chemical analysis with a dry basis, determined by a XEPOS X-ray fluorescence diffractometer (SPECTRO Analytical Instruments GmbH, Kleve, Germany) utilizing the X-LAB software, is given as oxides in wt % in Table 1. Loss on ignition was determined after heating perlite for 1 h at 1100 °C.
Fine raw perlite waste was measured on a MALVERN Laser Particle Size Analyzer with a mean particle size of d50: 26 μm. Its specific surface area was measured to be 0.65 m2/g by a QUANTACHROME Nova–1200 Ver 5.01 porosimeter (Boynton Beach, FL, USA). Its skeletal density, measured with a QUANTACHROME stereopycnometer, was 2402 kg/m3. The mineralogical analysis showed that the perlite waste was mostly amorphous, with only a small proportion of crystalline phases such as quartz and feldspars.
The alkaline activator that was used for the synthesis of geopolymer pastes was an aqueous sodium hydroxide solution, prepared by dissolving sodium hydroxide pellets (Merck Chemicals, Darmstadt, Germany, 99% purity) in deionized water.

2.2. Paste Preparation

The geopolymer viscous paste was prepared by mixing perlite with the alkaline activating solution for 20 min, until a homogeneous mixture was obtained. The NaOH concentration varied between 2 and 10 M, while the solid/liquid ratio was kept constant at 2 g/mL. The produced paste was cured under two different temperatures (70 °C and 90 °C).

2.3. Characterization Methods

Primarily, the setting time of geopolymer pastes was determined using a MATEST Vicat apparatus (Treviolo, Italy) in accordance with BS EN 196-3:2005+A1:2008 Methods of Testing Cement. Determination of setting times and soundness [21]. In addition, the dissolution of silicon from perlite in sodium hydroxide solution was studied in a 400-mL autoclave reactor, equipped with a thermostatically controlled heating mantle that was connected to a mercury contact thermometer, a mechanical stirrer with speed control, and a glass condenser. The dissolution tests were performed at 50, 70, and 90 °C for a 24-h retention time under intensive agitation, with a solid to liquid ratio (S/L) of 0.02–1 g/mL and a NaOH concentration of 2–6 M. At the end of each test, the suspension was filtered and the filtrate was further analyzed for its silicon content, using an inductively coupled plasma mass spectrometer (ICP–MS, Perkin Elmer, Waltham, MA, USA).

3. Results and Discussion

Characterization of Geopolymer Pastes Properties

The effect of the NaOH concentration on the setting time of geopolymer pastes was studied in the region from 2 M to 10 M. This characterization method is of high importance, as indicates the favorable conditions of the alkaline activator’s synthesis in the aqueous phase which contribute to the effective geopolymerization of perlite. The results are shown in Figure 1.
Figure 1 reveals that perlite geopolymer pastes solidify faster under lower NaOH solution concentrations, as well as at higher curing temperatures. More specifically, it is observed that 2 and 4 M NaOH solution constitute the optimum concentrations of the activator, at 90 °C, as the paste solidifies after 5 and 8 h, respectively. The former of the above observations is in contrast to the common perception that geopolymerization is most effective at high NaOH concentrations [22,23,24].
The setting time of the geopolymer pastes is affected by the SiO2/Na2O mass ratio, which controls the polycondensation phenomena in the aqueous phase, as indicated by the semi-quantitative interpretation of soluble silicate species (Figure 2).
The lower SiO2/Na2O mass ratios favor the formation of monomer and oligomer Si species [25,26,27], and therefore inhibit the polycondensation phenomena, slowing the setting time of perlite geopolymer pastes [27]. On the other hand, the higher SiO2/Na2O mass ratios favor the formation of large chains and complex polymer structures, indicating effective polycondensation phenomena as well as fast solidification of the pastes.
In order to define a suitable setting time of perlite pastes in low concentrations of the activator (as indicated by Figure 1 and Figure 2), the kinetic study of the SiO2/Na2O mass ratios at the aqueous phase of the geopolymer slurries was performed as a function of their stirring time at a constant solid to liquid ratio (S/L: 0.02 g/mL). The NaOH solution concentrations and the temperatures selected for this study were as follows: [NaOH]: 2–6 M, Temperature: 50–90 °C. The results are shown in Figure 3.
According to Figure 3a–c, it is observed that for each temperature, the SiO2/Na2O mass ratio increases inversely proportional to the concentration of NaOH solution in the aqueous phase. In addition, it is clearly seen that this ratio also increases as a function of the temperature, for the same alkalinity of solution and the same activation time, in accordance with similar studies of the literature [28,29,30,31,32]. Therefore, the higher curing temperatures of the geopolymer pastes as well as the lower NaOH concentrations of the solutions result in higher SiO2/Na2O mass ratios in the slurries. In this way, faster polycondensation is achieved, leading to a shorter setting time of the pastes (Figure 1).
Figure 3 also indicates that the highest SiO2/Na2O ratio, equal to 0.17 ([NaOH]: 2 M, Temperature: 90 °C), corresponds to the monosilicates and oligomers area of the semi-quantitative interpretation of soluble silicate species equilibria (Figure 2) [25,26,27]. This is possibly attributed to the low solid to liquid ratio of the geopolymer paste (S/L: 0.02 g/mL). Thus, an investigation of slurries with higher solid to liquid ratios was performed, in order to determine the real solid to liquid ratio of the geopolymer paste (S/L: 2 g/mL). The SiO2/Na2O mass ratio of the perlite pastes was studied at three different NaOH solution concentrations (2, 4, and 6 Μ) and three different solid to liquid ratios (0.2, 0.6, and 1 g/mL). The upper limit of the S/L ratio was equal to 1 g/mL due to the lack of the paste’s workability (due to the intensive agitation conditions under temperature) at higher ratios. Temperature was kept constant at 70 °C, which was considered to be the most appropriate choice for the mild curing of geopolymers. The results are shown in the diagrams below (Figure 4).
From Figure 4a–c, it is concluded that the increase of the pulp’s density at a constant concentration of NaOH solution leads to a higher SiO2/Na2O mass ratio in the aqueous phase of the slurry. According to Figure 4a, the highest SiO2/Na2O value (1.862 w/w) corresponds to the lowest concentration of NaOH solution in the aqueous phase (2 Μ NaOH), for the denser slurry (S/L: 1 g/mL) after 24 h of agitation at 70 °C. Slurries with 4 Μ NaOH solution concentration follow, reaching a SiO2/Na2O ratio equal to 1.683 w/w. Finally, the highest NaOH solution concentration slurries are observed with a value of 1.21 w/w. Therefore, it was found that the increased solid to liquid ratio of the geopolymer slurries results in higher SiO2/Na2O values, due to the efficient Si dissolution, promoting the polycondensation phenomena and rendering the geopolymerzation process.
In order for the SiO2/Na2O mass ratio of the real conditions in geopolymer slurries to be determined (S/L: 2 g/mL), a simple mathematical simulation of the experimental data shown in Figure 4 was employed. Thus, the mathematical trend of SiO2/Na2O mass evolution was determined in the solution, as a function of S/L ratio, for each value of stirring time that was studied (in order to obtain the necessary experimental data).
The mathematical equations used in all cases to adapt the experimental data is of the form:
y = a · xb,
  • y: SiO2/Na2O mass ratio;
  • x: solid to liquid ratio (S/L);
  • and a, b are constants.
The mathematical adaptation equations and their R2 values, on which the graphs of Figure 5 are based, are presented in Table 2.
Assuming that the mathematical adaption equations will apply to the case of S/L: 2 g/mL (no data support the truth of this hypothesis or not), by extrapolating the experimental data, the SiO2/Na2O values in the aqueous phase are obtained as a function of stirring time and NaOH solution concentration for S/L: 2 g/mL (Table 3 and Figure 6).
As shown in Figure 6, the SiO2/Na2O mass ratio at 70 °C for S/L: 2 g/mL is almost identical in the case of the alkaline solutions at concentrations of 2 and 4 M NaOH, while it is most noticeably lagging in the case of 6 M NaOH. This demonstrates the similar behavior of the alkaline solutions at 2 and 4 M NaOH under 70 °C with respect to the setting time of the pastes (Figure 1), explaining the delay of the slurry’s solidification under the highest concentration of the solution (6 M NaOH).

4. Conclusions

In this study, the efficient Si dissolution from perlite at alkaline solutions was determined, revealing high SiO2/Na2O mass ratios of the aqueous phase after treatment with low activator concentrations. The solid/liquid ratio was kept constant at 2 g/mL and the selected sodium hydroxide solution concentration varied between 2 and 10 M, presenting fast paste hardening at 70 °C and 90 °C for the low-level alkaline activator concentrations. Two series of dissolution tests were also performed at different NaOH concentrations, solid/liquid ratios, and temperature conditions, indicating that the actual amount of Si species that can be transferred into the solution is more than adequate, especially at low concentrations of NaOH solution (2 and 4 M NaOH). This makes them good potential raw materials for geopolymerization, a technology which could be ideally combined with appropriate foaming techniques for the production of lightweight insulating materials with a view to numerous applications in the construction field.

Author Contributions

Dimitrios Panias and Georgia-Maria Tsaousi conceived and designed the experiments; Georgia-Maria Tsaousi performed the experiments; Iliana Douni and Georgia-Maria Tsaousi analyzed the data; Georgia-Maria Tsaousi wrote the paper.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Barbosa, V.F.F.; MacKenzie, K.J.D.; Thaumatutgo, C. Synthesis and characterization of materials based on inorganic polymers of alumina and silica: Sodium polysialate polymers. Int. J. Inorg. Mater. 2000, 4, 309–317. [Google Scholar] [CrossRef]
  2. Xu, H.; Van Deventer, J.S.J. The geopolymerization of alumino-silicate minerals. Int. J. Miner. Process. 2000, 3, 247–266. [Google Scholar] [CrossRef]
  3. Palomo, A.; Grutzeck, M.W.; Blanco, M.T. Alkali activated fly ashes-a cement for the future. Cem. Concr. Res. 1999, 8, 1323–1329. [Google Scholar] [CrossRef]
  4. Palomo, A.; Krivenko, P.; Garcia-Lodeiro, I.; Kavalerova, E.; Maltseva, O.; Fernández-Jiménez, A. A review on alkaline activation: New analytical perspectives. Mater. Construc. 2014, 64, e022. [Google Scholar] [CrossRef]
  5. Cheng, T.W.; Chiu, J.P. Fire resistant Geopolymer produced by granulated blast furnace slag. Miner. Eng. 2003, 3, 205–210. [Google Scholar] [CrossRef]
  6. Cundi, W.; Hirano, Y.; Terai, T.; Vallepu, R.; Mikuni, A.; Ikeda, K. Preparation of geopolymeric monoliths from red mud-PFBC ash fillers at ambient temperature. In Proceedings of the World Congress Geopolymer, Saint Quentin, France, 28 June–1 July 2005; pp. 85–87. [Google Scholar]
  7. Panias, D.; Giannopoulou, I.; Perraki, T. Effect of synthesis parameters on the mechanical properties of fly ash-based geopolymers. Colloids Surf. A 2007, 301, 246–254. [Google Scholar] [CrossRef]
  8. Maragos, I.; Giannopoulou, I.; Panias, D. Synthesis of ferronickel slag-based geopolymers. Miner. Eng. 2008, 22, 196–203. [Google Scholar] [CrossRef]
  9. Pontikes, Y.; Machiels, L.; Onisei, S.; Pandelaers, L.; Geysen, D.; Jones, P.T.; Blanpain, B. Slags with a high Al and Fe content as precursors for inorganic polymers. Appl. Clay Sci. 2013, 73, 93–102. [Google Scholar] [CrossRef]
  10. Komnitsas, K.; Zaharaki, D.; Perdikatsis, V. Effect of synthesis parameters on the compressive strength of low-calcium ferronickel slag inorganic polymers. J. Hazard. Mater. 2009, 161, 760–768. [Google Scholar] [CrossRef] [PubMed]
  11. Barbosa, V.F.F.; MacKenzie, K.J.D. Thermal behavior of inorganic geopolymers and composites derived from sodium polysialate. Mater. Res. Bull. 2003, 38, 319–331. [Google Scholar] [CrossRef]
  12. Davidovits, J. Properties of geopolymer cements. In Proceedings of the First International Conference on Alkaline Cements and Concretes, Geopolymer Institute, Kiev, Ukraine, 11–14 October 1994; pp. 131–149. [Google Scholar]
  13. Swanepoel, J.C.; Strydom, C.A. Utilization of fly ash in a geopolymeric material. Appl. Geochem. 2002, 17, 1143–1148. [Google Scholar] [CrossRef]
  14. Nicholson, C.; Fletcher, R.; Miller, N.; Stirling, C.; Morris, J.; Hodges, S.; MacKenzie, K.; Schmücker, M. Building Innovation through Geopolymer Technology. Chem. N. Z. 2005, 69, 10–12. [Google Scholar]
  15. Ryu, G.S.; Lee, Y.B.; Koh, K.T.; Chung, Y.S. The mechanical properties of fly ash-based geopolymer concrete with alkaline activators. Constr. Build. Mater. 2013, 47, 409–418. [Google Scholar] [CrossRef]
  16. Vaou, V.; Panias, D. Thermal insulating foamy geopolymers from perlite. Miner. Eng. 2010, 23, 1146–1151. [Google Scholar] [CrossRef]
  17. Sakkas, K.; Nomikos, P.; Sofianos, A.; Panias, D. Sodium-based fire resistant geopolymer for passive fire protection. Fire Mater. 2014a, 39, 259–270. [Google Scholar] [CrossRef]
  18. Sakkas, K.; Panias, D.; Nomikos, P.; Sofianos, A. Potassium based geopolymer for passive fire protection of concrete tunnels linings. Tunn. Undergr. Space Technol. 2014b, 43, 148–156. [Google Scholar] [CrossRef]
  19. Erdogan, S. Properties of Ground Perlite Geopolymer Mortars. J. Mater. Civ. Eng. 2014, 27. [Google Scholar] [CrossRef]
  20. U.S. Geological Survey. Mineral Commodity Summaries; U.S. Geological Survey: Reston, VA, USA, 2016.
  21. BSI Standards Publication. Methods of Testing Cement. Determination of Setting Times and Soundness; British Standards Institute: London, UK, 2005. [Google Scholar]
  22. Giannopoulou, I.; Dimas, D.; Maragos, I.; Panias, D. Utilization of metallurgical solid wastes/by-products for development of inorganic polymeric construction materials. Glob. NEST J. 2009, 11, 127–136. [Google Scholar]
  23. Rattanasak, U.; Chindaprasirt, P. Influence of NaOH solution on the synthesis of fly ash geopolymer. Miner. Eng. 2009, 22, 1073–1078. [Google Scholar] [CrossRef]
  24. Panagiotopoulou, Ch.; Kontori, E.; Perraki, Th.; Kakali, G. Dissolution of aluminosilicate minerals and by-products in alkaline media. J. Mater. Sci. 2007, 42, 2967–2973. [Google Scholar] [CrossRef]
  25. PQ Corporation Industrial Chemical Division—National Silicates, Fundamentals of Silicate Chemistry. Available online: http://www.pqcorp.com/corporate/aboutpq.asp (accessed on 6 April 2006).
  26. Gerke, H.; Gies, H.; Liebau, F. Tetrabutylammonium hydrogen silicate: synthesis, chemical, thermal, and crystallographic properties. In Soluble Silicates; ACS Symposium Series 194; Falcone, J.S., Jr., Ed.; ACS Publications: Washington, DC, USA, 1982; pp. 305–318. [Google Scholar]
  27. Duxson, P.; Provis, J.; Lukey, G.; Mallicoat, S.; Kriven, W.; Van Deventer, J. Understanding the relationship between geopolymer composition, microstructure and mechanical properties. Colloids Surf. A 2005, 269, 47–58. [Google Scholar] [CrossRef]
  28. Fertani, M.; Brahim, K.; Khattech, I.; Jemal, M. Thermochemistry and kinetics of silica dissolution in NaOH solutions: Effect of the alkali concentration. Thermochim. Acta 2014, 594, 58–67. [Google Scholar] [CrossRef]
  29. Srivastava, K.; Shringi, N.; Devra, V.; Rani, A. Pure silica extraction from perlite: Its characterization and affecting factors. Int. J. Innov. Res. Sci. Eng. Technol. 2013, 2, 2936–2942. [Google Scholar]
  30. Niibori, Y.; Kunita, M.; Tochiyama, O.; Chida, T. Dissolution rates of amorphous silica in highly alkaline solution. J. Nucl. Sci. Technol. 2000, 37, 349–357. [Google Scholar] [CrossRef]
  31. Adam, G.; Carr, A.; Tester, J.W. Prediction of the solubility of quartz in salt solutions from 25–900 °C using the 3-parameter Non-Random Two liquid (NRTL) model. Fluid Ph. Equilib. 2013, 337, 288–297. [Google Scholar]
  32. Brady, P.V.; Walther, J.V. Controls on silicate dissolution rates in neutral and basic pH at 25 °C. Geochim. Acta 1989, 53, 2822–2830. [Google Scholar] [CrossRef]
Figure 1. Setting time of geopolymer paste as a function of NaOH concentration (S/L: 2 g/mL, Temperature: 70 and 90 °C).
Figure 1. Setting time of geopolymer paste as a function of NaOH concentration (S/L: 2 g/mL, Temperature: 70 and 90 °C).
Minerals 08 00160 g001
Figure 2. Semi-quantitative interpretation of soluble silicate species equilibria in 1 m aqueous silicate solution (Reproduced from Reference [25]).
Figure 2. Semi-quantitative interpretation of soluble silicate species equilibria in 1 m aqueous silicate solution (Reproduced from Reference [25]).
Minerals 08 00160 g002
Figure 3. SiO2/Na2O mass ratio (w/w) in the aqueous phase of geopolymer slurries as a function of stirring time and the concentration of NaOH solution at three different temperatures: (a) 90 °C; (b) 70 °C; (c) 50 °C ([NaOH]: 2, 4, and 6 M, S/L: 0.02 g/mL).
Figure 3. SiO2/Na2O mass ratio (w/w) in the aqueous phase of geopolymer slurries as a function of stirring time and the concentration of NaOH solution at three different temperatures: (a) 90 °C; (b) 70 °C; (c) 50 °C ([NaOH]: 2, 4, and 6 M, S/L: 0.02 g/mL).
Minerals 08 00160 g003
Figure 4. SiO2/Na2O mass ratio (w/w) in the aqueous phase of geopolymer slurries as a function of stirring time at different concentrations of NaOH solution: (a) 2 Μ; (b) 4 Μ; (c) 6 Μ (Temperature: 70 °C, S/L: 0.02–1 g/mL).
Figure 4. SiO2/Na2O mass ratio (w/w) in the aqueous phase of geopolymer slurries as a function of stirring time at different concentrations of NaOH solution: (a) 2 Μ; (b) 4 Μ; (c) 6 Μ (Temperature: 70 °C, S/L: 0.02–1 g/mL).
Minerals 08 00160 g004
Figure 5. Graphical representation of the mathematical equations employed to adapt the experimental data of Figure 4 in three different NaOH solution’s concentrations: (a) 2 M NaOH; (b) 4 M NaOH; (c) 6 M NaOH.
Figure 5. Graphical representation of the mathematical equations employed to adapt the experimental data of Figure 4 in three different NaOH solution’s concentrations: (a) 2 M NaOH; (b) 4 M NaOH; (c) 6 M NaOH.
Minerals 08 00160 g005
Figure 6. Prediction of SiO2/Na2O mass ratio in the alkaline activator for geopolymer slurries with S/L: 2 g/mL at 70 °C as a function of stirring time and NaOH solution concentration (2–6 M).
Figure 6. Prediction of SiO2/Na2O mass ratio in the alkaline activator for geopolymer slurries with S/L: 2 g/mL at 70 °C as a function of stirring time and NaOH solution concentration (2–6 M).
Minerals 08 00160 g006
Table 1. Chemical analysis of perlite waste.
Table 1. Chemical analysis of perlite waste.
Oxides (%) w/w
Na2OMgOAl2O3SiO2K2OCaOFe2O3LOITOTAL
3.990.2710.5175.334.311.381.172.83100
Table 2. Mathematical data adaptation equations from Figure 5.
Table 2. Mathematical data adaptation equations from Figure 5.
Time, h2 M NaOH4 M NaOH6 M NaOH
EquationR2EquationR2EquationR2
1y = 0.2398 x0.62820.9895y = 0.2627 x0.65920.8797y = 0.0716 x0.47980.8892
3y = 0.2927 x0.49640.9786y = 0.3162 x0.59440.9625y = 0.1651 x0.62440.9021
5y = 0.422 x0.5190.9926y = 0.4598 x0.60720.9844y = 0.2925 x0.64340.9974
7y = 0.5128 x0.4870.9994y = 0.6581 x0.68580.9948y = 0.4007 x0.67530.9964
24y = 2.0605 x0.67720.9959y = 1.939 x0.73450.9843y = 1.3525 x0.72370.9947
Table 3. Prediction of SiO2/Na2O mass ratio in the alkaline activator for geopolymer slurries with S/L: 2 g/mL as a function of stirring time and NaOH solution concentration, at 70 °C.
Table 3. Prediction of SiO2/Na2O mass ratio in the alkaline activator for geopolymer slurries with S/L: 2 g/mL as a function of stirring time and NaOH solution concentration, at 70 °C.
Time, h2 M NaOH4 M NaOH6 M NaOH
SiO2/Na2O, w/wSiO2/Na2O, w/wSiO2/Na2O, w/w
10.37060.41490.0999
30.41290.47750.2545
50.60470.70040.4569
70.71881.05860.6399
243.29483.22622.2335

Share and Cite

MDPI and ACS Style

Tsaousi, G.-M.; Douni, I.; Panias, D. Experimental Evaluation of Efficient Si Dissolution from Perlite at Low Level Activator’s Concentration. Minerals 2018, 8, 160. https://0-doi-org.brum.beds.ac.uk/10.3390/min8040160

AMA Style

Tsaousi G-M, Douni I, Panias D. Experimental Evaluation of Efficient Si Dissolution from Perlite at Low Level Activator’s Concentration. Minerals. 2018; 8(4):160. https://0-doi-org.brum.beds.ac.uk/10.3390/min8040160

Chicago/Turabian Style

Tsaousi, Georgia-Maria, Iliana Douni, and Dimitrios Panias. 2018. "Experimental Evaluation of Efficient Si Dissolution from Perlite at Low Level Activator’s Concentration" Minerals 8, no. 4: 160. https://0-doi-org.brum.beds.ac.uk/10.3390/min8040160

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop