Recycling Lithium from Waste Lithium Bromide to Produce Lithium Hydroxide
Next Article in Special Issue
A Novel Nitrogen Ion Implantation Technique for Turning Thin Film “Normally On” AlGaN/GaN Transistor into “Normally Off” Using TCAD Simulation
Previous Article in Journal
The Natural Oligoribonucleotides Functionalized by D-Mannitol Affected Interactions of Hemagglutinin with Glycan Receptor Indicating Anti-Influenza Activity
Previous Article in Special Issue
Application of Amorphous Zirconium-Yttrium-Aluminum-Magnesium-Oxide Thin Film with a High Relative Dielectric Constant Prepared by Spin-Coating
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Communication

Improvements of Electrical Characteristics in Poly-Si Nanowires Thin-Film Transistors with External Connection of a BiFeO3 Capacitor

1
Department of Electronic Engineering, Feng Chia University, Taichung 407, Taiwan
2
Department of Electrical Engineering, National Chung Hsing University, Taichung 407, Taiwan
3
Department of Electrical Engineering, Hsiuping University of Science and Technology, Taichung 407, Taiwan
*
Author to whom correspondence should be addressed.
Submission received: 6 September 2021 / Revised: 23 September 2021 / Accepted: 29 September 2021 / Published: 30 September 2021
(This article belongs to the Special Issue Thin-Film Transistors)

Abstract

:
By a sol–gel method, a BiFeO3 (BFO) capacitor is fabricated and connected with the control thin film transistor (TFT). Compared with a control thin-film transistor, the proposed BFO TFT achieves 56% drive current enhancement and 7–28% subthreshold swing (SS) reduction. Moreover, the effect of the proposed BiFeO3 capacitor on IDS-VGS hysteresis in the BFO TFT is 0.1–0.2 V. Because dVint/dVGS > 1 is obtained at a wide range of VGS, it reveals that the incomplete dipole flipping is a major mechanism to obtain improved SS and a small hysteresis effect in the BFO TFT. Experimental results indicate that sol-gel BFO TFT is a potential candidate for digital application.

1. Introduction

Recently, negative capacitance (NC) transistors have been widely studied, because they are considered to be one of the most promising candidates for low power applications. The NC transistor is first proposed by Salahuddin and Datta. In NC transistors, an embedded ferroelectric film in the gate stack plays a role of voltage amplification [1]. Many studies have been demonstrated transistor integrated with various ferroelectrics, such as HfZrOx [2,3,4,5,6,7], PbZrTiO3 [8,9], PVDF [10,11], and BiFeO3 (BFO) [12]. NC transistors are expected to be applied for logic switching, which requires hysteresis-free characteristics. Generally, the phenomena of clockwise hysteresis show their NC effect. Some studies reveal that a complete dipole flipping in ferroelectric can obtain a large hysteresis, but an incomplete dipole flipping in ferroelectric can obtain a small hysteresis [13,14,15]. BFO is a single phase multiferroic material with a rhombohedrally distorted perovskite with polar space group R3c at room temperature [16]. Although BFO is a very good ferroelectric material, it is still not widely used in negative capacitance transistors. In reference [12], although BFO negative capacitance transistors can achieve a very low subthreshold swing (SS) from 8.5 to 50 mV/decade, the effect of BFO capacitor on the hysteresis is about 4–5 V. Therefore, as far as digital applications are concerned, more studies are needed for BFO negative capacitance transistors. In this paper, BFO thin film on Pt will be fabricated by a low-cost sol–gel method [17] and the Poly-Si nanowire junctionless thin film transistor (TFT) externally connected to the BFO capacitor will be investigated. Interestingly, our results reveal that the incomplete dipole flipping in the BFO capacitor plays a major role to obtain a small hysteresis effect in the proposed BFO TFT device.

2. Devices Fabrication

A 100-nm-thick in-situ phosphorus-doped (N+) Poly-Si was deposited on oxidized silicon wafer by low-pressure chemical vapor deposition (LPCVD). The 100-nm-thick Poly-Si was then patterned, using partial etching to form one 50-nm-thick Poly-Si strip, as shown in Figure 1a. Then, a 20-nm-thick Si3N4 film was deposited by LPCVD, as shown in Figure 1b. Next, a 15-nm-thick N+ Poly-Si was deposited by LPCVD at 560 °C and then annealed at 600 °C for 10 hours, which recrystallized it into Poly-Si through solid-phase crystallization. Then, using standard I-line lithography, the photoresists on the source/drain (S/D) pads were patterned to overlap on the two edges of the raised strip. After that, a plasma etcher was used to remove the N+ Poly-Si, while the spacer Si channels were formed on the sidewall of each L-type Si3N4 film, in situ, and naturally connected to the S/D pads, as shown in Figure 1c. Next, S/D-pad photoresists were removed and 5-nm-thick atomic layer deposition (ALD). Al2O3 and 100-nm-thick TiN were deposited by sputtering system as the gate oxide and the gate electrode, as shown in Figure 1d. The schematic cross-sectional channel and its TEM image were shown in Figure 1e,f. In this paper, the main purpose is to study the influence of BiFeO3 (BFO) capacitor on the characteristics of transistors. Therefore, the process of control transistors used in the paper is not optimized.
For BiFeO3 capacitors, BFO thin film was fabricated on Pt/Ti/SiO2/Si by a sol–gel method. Bismuth (III) acetate [Bi(OOCCH3)3] and Iron(III) 2,4-pentanedionate [C15H21FeO6] were used as raw materials. These starting materials were first dissolved in propionic acid and 2-methoxyethanol with Bi excess 5%. The solution was then stirred at 80 °C for 4h to obtain a uniform sol solution, and was subsequently coated in Pt/Ti/SiO2/Si substrate with 2500 rpm for 30 s and dried at 300 °C for 2 min. This step was repeated 10 times to obtain the final BFO films (~300 nm). The BFO film was annealed at 550 °C for 30s and called 550-BFO. Finally, Al were deposited by sputtering as with the top gate, as shown in Figure 1g. A wire was connected to the 550-BFO capacitor and control TFT, as shown in Figure 1h. All upper electrodes were circular, and a BFO capacitor with a radius of 170 μm was used in the study of the NC effect in the resistive–capacitive (RC) circuit, and the BFO capacitor with a radius of 28um was connected in series with the control transistor. The size of the control TFT is Weff = 30 nm × 2/L = 5 μm in the proposed 550-BFO TFT.

3. Results and Discussion

For BFO film, the grain structure of the film was detected using a scanning electron microscope (SEM), as shown in Figure 2a. The 550-BFO film shows relatively obvious grains. It reveals that the BFO film annealed at 550 °C is well crystallized. XRD patterns of the BFO film annealed at 550 °C is shown in Figure 2b and the (012), (110), (104), (024), (122), (300), and (214) diffraction peaks can be observed. The XRD peaks are quite similar to those of standard diffraction patterns of pure BFO on the joint committee on powder diffraction standards (JCPDS #71-2494) card. This indicates the formation of pure BFO phase, good crystallization, and rhombohedrally-distorted perovskite crystal structure with space group R3c [18]. According to the previous study, it reveals that the proposed 550-BFO film has good ferroelectric properties [18].
To study the NC effect, we created an RC circuit diagram of the experimental setup where the 550-BFO capacitor is connected in series with an external resistor Rs = 500 Ω, as shown in Figure 3a. An AC voltage pulse sequence of Vs: −5V → +5V → −5V was applied as input and the voltage (VF) across the BFO capacitor was recorded by an oscilloscope. Figure 3b shows the transient response of VF from −5V to +5V and from +5V to −5V for the 550-BFO capacitor. In Figure 3b, the spike behavior can be understood in the following sequence: initial rise, initial ferroelectric response, and final ferroelectric response. According to reference [12], the NC time is defined the elapsed time from the highest value (or lowest value) to the lowest value (or highest value) of VF in “initial ferroelectric response” and a longer NC time shows a longer charge compensation time after domain switching. Obviously, for the positive domain switching, the NC time is 0.160 μs and 0.136 μs for the negative domain switching. Therefore, whether with forward- or reverse sweeping, it is expected that the characteristics of 550-BFO TFT will be improved over the control TFT.
The IDS-VGS transfer characteristics at VDS of 0.1 V and 2 V for control TFT and 550-BFO TFT are shown in Figure 4b, respectively. The VTH is defined as the gate voltage that is required to obtain a normalized drain current of IDS = (Weff/L) × 10−8 A. For 550-BFO TFT, the hysteresis from 0.59 V to 0.45 V at VDS of 0.1 V is observed, as shown in Figure 4a. At VDS of 2 V, the hysteresis from 0.6 V to 0.4 V is observed, as shown in Figure 4b. From the hysteresis curves, the effect of the 550-BFO capacitor on hysteresis is about 0.14 V and 0.2 V at 0.1 V and VDS of 2 V, respectively. For 550-BFO TFT, no matter at VDS of 0.1 V or 2 V, the ON current (ION) at VGS of 3 V shows 56% enhancement over control TFT.
Figure 5a,b shows the point SS versus IDS curves for control TFT and 550-BFO TFT. Compared with control TFT, no matter forward sweeping or reverse sweeping, 550-BFO TFT show improved SS characteristics at VDS of 0.1 V or 2 V over control TFT. In the IDS range of 1 × 108 to 1 × 1011 A, the average SS value is reduced by 28% for forward sweeping and 7% for reverse sweeping. The SS data is consistent with the trend of NC time of positive and negative domain switching. Based on the assumption that the IDS of 550-BFO TFT is the same as the control TFT, the extracted Vint-VGS curve at VDS of 0.1V can be obtained [15]. dVint/dVGS versus VGS can be calculated, as shown in Figure 5c. It is found that dVint/dVGS > 1 is obtained at a wide range of VGS, leading to the improved SS over control TFT in the whole measuring range of IDS in 550-BFO TFT. The previous study reported that the mechanism underlying near IDS-VGS hysteresis-free transistor is incomplete dipoles flipping, rather than complete dipoles switching in the transistor with a large IDS-VGS hysteresis [15]. Therefore, the incomplete dipole flipping plays a major role to obtain improved SS and a small hysteresis effect in the proposed 550-BFO TFT. According to the data and discussion mentioned above, it reveals that sol-gel BFO TFT is a potential candidate for digital application.

4. Conclusions

The proposed BFO TFT shows improved characteristics of ION increased by 56% and SS reduced by 7–28%, because the sol gel BFO film show good crystallization, ferroelectric property, and a long enough NC time. Based on the extracted Vint-VGS curve, dVint/dVGS > 1 is obtained at a wide range of VGS. Obviously, the incomplete dipole flipping plays a major role in the proposed BFO TFT. Therefore, the effect of the proposed BFO capacitor on IDS-VGS hysteresis in the BFO TFT is small. It reveals that the proposed BFO TFT is a potential candidate for digital application.

Author Contributions

Conceptualization, T.-K.K.; formal analysis, T.-K.K., Y.-Y.L., C.-L.L. and P.-J.C.; methodology, T.-K.K., M.-C.K. and H.-Z.C.; resources, T.-K.K., M.-C.K. and H.-Z.C.; writing—original draft, T.-K.K. and H.-W.L.; writing—review and editing, T.-K.K., H.-W.L. and M.-C.K. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Ministry of Science and Technology of Taiwan (grant MOST no. MOST.108-2221-E-035-040).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Salahuddin, S.; Datta, S. Use of negative capacitance to provide voltage amplification for low power nanoscale devices. Nano Lett. 2008, 8, 405–410. [Google Scholar] [CrossRef] [PubMed]
  2. Li, K.S.; Chen, P.G.; Lai, T.Y.; Lin, C.H.; Cheng, C.C.; Chen, C.C.; Wei, Y.J.; Hou, Y.F.; Liao, M.H.; Lee, M.H.; et al. Sub-60mV-swing negative-capacitance FinFET without hysteresis. In Proceedings of the 2015 IEEE International Electron Devices Meeting (IEDM), Washington, DC, USA, 7–9 December 2015; pp. 620–623. [Google Scholar]
  3. Lee, M.H.; Wei, Y.-T.; Chu, K.-Y.; Huang, J.-J.; Chen, C.-W.; Cheng, C.-C.; Chen, M.-J.; Lee, H.-Y.; Chen, Y.-S.; Lee, L.-H.; et al. Steep slope and near non-hysteresis of FETs with antiferroelectric-like HfZrO for low-power electronics. IEEE Electron Device Lett. 2015, 36, 294–296. [Google Scholar] [CrossRef]
  4. Cheng, C.H.; Chin, A. Low-voltage steep turn-on pMOSFET using ferroelectric high-κ gate dielectric. IEEE Electron Device Lett. 2014, 35, 274–276. [Google Scholar] [CrossRef]
  5. Lee, M.H.; Chen, P.-G.; Liu, C.; Chu, K.-Y.; Cheng, C.-C.; Xie, M.-J.; Liu, S.-N.; Lee, J.-W.; Huang, S.-J.; Liao, M.-H.; et al. Prospects for ferroelectric HfZrOx FETs with experimentally CET = 0.98 nm, SSfor = 42mV/dec, SSrev =28mV/dec, switch-OFF <0.2V, and hysteresis-free strategies. In Proceedings of the 2015 IEEE International Electron Devices Meeting (IEDM), Washington, DC, USA, 7–9 December 2015; pp. 616–619. [Google Scholar]
  6. Zhou, J.; Han, G.; Li, Q.; Peng, Y.; Lu, X.; Zhang, C.; Zhang, J.; Sun, Q.-Q.; Zhang, D.W.; Hao, Y. Ferroelectric HfZrOx Ge and GeSn pMOSFETs with sub-60 mV/decade subthreshold swing, negligible hysteresis, and improved IDS. In Proceedings of the 2016 IEEE International Electron Devices Meeting (IEDM), San Francisco, CA, USA, 3–7 December 2016; pp. 310–313. [Google Scholar]
  7. Zhou, J.; Han, G.; Peng, Y.; Liu, Y.; Zhang, J.; Sun, Q.-Q.; Zhang, D.W.; Hao, Y. Ferroelectric negative capacitance GeSn PFETs with sub-20 mV/decade subthreshold swing. IEEE Electron Device Lett. 2017, 38, 1157–1160. [Google Scholar] [CrossRef]
  8. Dasgupta, S.; Rajashekhar, A.; Majumdar, K.; Agrawal, N.; Razavieh, A.; Trolier-Mckinstry, S.; Datta, S. Sub-kT/q switching in strong inversion in PbZr0.52Ti0.48O3 gated negative capacitance FETs. IEEE J. Explor. Solid-State Comput. Devices Circuits 2015, 1, 43–48. [Google Scholar] [CrossRef]
  9. Bakaul, S.R.; Serrao, C.R.; Lee, M.; Yeung, C.W.; Sarker, A.; Hsu, S.-L.; Yadav, A.; Dedon, L.; You, L.; Khan, A.I.; et al. Single crystal functional oxides on silicon. Nat. Commun. 2016, 7, 10547. [Google Scholar] [CrossRef] [PubMed]
  10. Rusu, A.; Salvatore, G.A.; Jiménez, D.; Ionescu, A.M. Metal ferroelectric-meta-oxide-semiconductor field effect transistor with sub-60mV/decade subthreshold swing and internal voltage amplification. In Proceedings of the 2010 International Electron Devices Meeting, San Francisco, CA, USA, 6–8 December 2010; pp. 395–398. [Google Scholar]
  11. Jo, J.; Shin, C. Negative capacitance field effect transistor with hysteresis-free sub-60-mV/decade switching. IEEE Electron Device Lett. 2016, 37, 245–248. [Google Scholar] [CrossRef]
  12. Khan, A.I.; Chatterjee, K.; Duarte, J.P.; Lu, Z.; Sachid, A.; Khandelwal, S.; Ramesh, R.; Hu, C.; Salahuddin, S. Negative capacitance in short-channel FinFETs externally connected to an epitaxial ferroelectric capacitor. IEEE Electron Device Lett. 2016, 37, 111–114. [Google Scholar] [CrossRef]
  13. Jia, C.-L.; Urban, K.W.; Alexe, M.; Hesse, D.; Vrejoiu, I. Direct observation of continuous electric dipole rotation in flux-closure domains in ferroelectric Pb(Zr,Ti)O3. Science 2011, 331, 1420–1433. [Google Scholar] [CrossRef] [PubMed]
  14. Naumov, I.; Bratkovsky, A.M. Unusual polarization patterns in flat epitaxial ferroelectric nanoparticles. Phys. Rev. Lett. 2008, 10, 107601. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  15. Zhou, J.; Han, G.; Xu, N.; Li, J.; Peng, Y.; Liu, Y.; Zhang, J.; Sun, Q.Q.; Zhang, D.W.; Hao, Y. Incomplete Dipole Flipping Produced Near Hystersis-Free Negative Capacitance Transistor. IEEE Electron Device Lett. 2019, 40, 329–332. [Google Scholar] [CrossRef]
  16. Quan, Z.C.; Hu, H.; Xu, S.; Liu, W.; Fang, G.; Li, M.; Zhao, X. Surface chemical bonding states and ferroelectricity of Ce-doped BiFeO3 thin films prepared by sol-gel process. J. Sol-Gel Sci. Technol. 2008, 48, 261–266. [Google Scholar] [CrossRef]
  17. Wang, D.; Wang, M.; Liu, F.; Cui, Y.; Zhao, Q.; Sun, H.; Jin, H.; Cao, M. Sol-gel synthesis of Nd-doped BiFeO3 multiferroic and its characterization. Ceram. Int. 2015, 41, 8768–8772. [Google Scholar] [CrossRef]
  18. Anjum, T.A.; Naveed-Ul-Haq, M.; Hussain, S.; Rafique, M. Analyses of structure, electronic and multiferroic properties of Bi1−xNdxFeO3 (x = 0, 0.05, 0.10, 0.15, 0.20, 0.25) system. J. Alloy. Compd. 2020, 820, 153095. [Google Scholar] [CrossRef]
Figure 1. Key fabrication steps for the control TFT and BFO capacitor. (a) N+ Poly-Si layer deposition and strip patterning, (b) Si3N4 deposition, (c) N+ Poly-Si layer deposition, N+ Poly-Si NW channels and source/drain were Figure 2. (d) O3 gate oxide and TiN deposition, then gate patterning, (e) the cross-sectional transistor with TiN gate, (f) the cross-sectional TEM image, where the red line indicates the Si channel. Its peripheries are 9.4 nm, 24 nm, and 35 nm, respectively. Due to 5-nm-thick Al2O3, the effective width (Weff)/channel of TiN gate is about 30nm in control TFT. (g) Schematic diagram of BFO capacitor. (h) A wire is connected to the BFO capacitor and a control transistor where it can be measured.
Figure 1. Key fabrication steps for the control TFT and BFO capacitor. (a) N+ Poly-Si layer deposition and strip patterning, (b) Si3N4 deposition, (c) N+ Poly-Si layer deposition, N+ Poly-Si NW channels and source/drain were Figure 2. (d) O3 gate oxide and TiN deposition, then gate patterning, (e) the cross-sectional transistor with TiN gate, (f) the cross-sectional TEM image, where the red line indicates the Si channel. Its peripheries are 9.4 nm, 24 nm, and 35 nm, respectively. Due to 5-nm-thick Al2O3, the effective width (Weff)/channel of TiN gate is about 30nm in control TFT. (g) Schematic diagram of BFO capacitor. (h) A wire is connected to the BFO capacitor and a control transistor where it can be measured.
Membranes 11 00758 g001
Figure 2. (a) SEM image of BFO film annealed at 550 °C. (b) XRD pattern of BFO film annealed at 550 °C.
Figure 2. (a) SEM image of BFO film annealed at 550 °C. (b) XRD pattern of BFO film annealed at 550 °C.
Membranes 11 00758 g002
Figure 3. (a) Schematic diagram of experimental setup where the BFO capacitor is connected in series with a resistor (RC circuit). The pulse time is 25 μs. In the zoom, the solid line represents the input Vs signal and the dotted line represents the output voltage of the BFO capacitor. (b) Transient response of VF for BFO capacitor. The NC time is 0.160 μs from −5 V to 5 V and 0.136 μs from 5 V to −5 V.
Figure 3. (a) Schematic diagram of experimental setup where the BFO capacitor is connected in series with a resistor (RC circuit). The pulse time is 25 μs. In the zoom, the solid line represents the input Vs signal and the dotted line represents the output voltage of the BFO capacitor. (b) Transient response of VF for BFO capacitor. The NC time is 0.160 μs from −5 V to 5 V and 0.136 μs from 5 V to −5 V.
Membranes 11 00758 g003
Figure 4. (a) IDS-VGS transfer characteristics at VDS of 0.1 V for control TFT (L = 5 μm, Weff = 60 nm) and 550-BFO TFT. (b) IDS-VGS transfer characteristics at VDS of 2 V for control TFT and 550-BFO TFT.
Figure 4. (a) IDS-VGS transfer characteristics at VDS of 0.1 V for control TFT (L = 5 μm, Weff = 60 nm) and 550-BFO TFT. (b) IDS-VGS transfer characteristics at VDS of 2 V for control TFT and 550-BFO TFT.
Membranes 11 00758 g004
Figure 5. Point SS versus IDS curves for (a) control TFT (L = 5 μm, Weff = 60 nm) and 550-BFO TFT at VDS of 0.1 V and (b) at VDS of 2 V. (c) Extracted Vint and dVint/dVGS versus VGS at VDS of 0.1 V. The position of VGS and Vint are marked in Figure 1h.
Figure 5. Point SS versus IDS curves for (a) control TFT (L = 5 μm, Weff = 60 nm) and 550-BFO TFT at VDS of 0.1 V and (b) at VDS of 2 V. (c) Extracted Vint and dVint/dVGS versus VGS at VDS of 0.1 V. The position of VGS and Vint are marked in Figure 1h.
Membranes 11 00758 g005
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Kang, T.-K.; Lin, Y.-Y.; Liu, H.-W.; Lin, C.-L.; Chang, P.-J.; Kao, M.-C.; Chen, H.-Z. Improvements of Electrical Characteristics in Poly-Si Nanowires Thin-Film Transistors with External Connection of a BiFeO3 Capacitor. Membranes 2021, 11, 758. https://0-doi-org.brum.beds.ac.uk/10.3390/membranes11100758

AMA Style

Kang T-K, Lin Y-Y, Liu H-W, Lin C-L, Chang P-J, Kao M-C, Chen H-Z. Improvements of Electrical Characteristics in Poly-Si Nanowires Thin-Film Transistors with External Connection of a BiFeO3 Capacitor. Membranes. 2021; 11(10):758. https://0-doi-org.brum.beds.ac.uk/10.3390/membranes11100758

Chicago/Turabian Style

Kang, Tsung-Kuei, Yu-Yu Lin, Han-Wen Liu, Che-Li Lin, Po-Jui Chang, Ming-Cheng Kao, and Hone-Zern Chen. 2021. "Improvements of Electrical Characteristics in Poly-Si Nanowires Thin-Film Transistors with External Connection of a BiFeO3 Capacitor" Membranes 11, no. 10: 758. https://0-doi-org.brum.beds.ac.uk/10.3390/membranes11100758

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop