Article

The Effect of Boron on the Microstructure and Properties of Refractory Metal Intermetallic Composites (RM(Nb)ICs) Based on Nb-24Ti-xSi (x = 16, 17 or 18 at.%) with Additions of Al, Cr or Mo

by
Tophan Thandorn
1,2 and
Panos Tsakiropoulos
2,*
1
Department of Materials Science and Engineering, School of Science, Mae Fah Luang University, Chiang Rai 57100, Thailand
2
Department of Materials Science and Engineering, Sir Robert Hadfield Building, The University of Sheffield, Sheffield S1 3JD, UK
*
Author to whom correspondence should be addressed.
Submission received: 21 August 2021 / Revised: 27 September 2021 / Accepted: 4 October 2021 / Published: 15 October 2021

Abstract

:
This paper is about metallic ultra-high temperature materials, in particular, refractory metal intermetallic composites based on Nb, i.e., RM(Nb)ICs, with the addition of boron, which are compared with refractory metal high entropy alloys (RHEAs) or refractory metal complex concentrated alloys (RCCAs). We studied the effect of B addition on the density, macrosegregation, microstructure, hardness and oxidation of four RM(Nb)IC alloys, namely the alloys TT2, TT3, TT4 and TT8 with nominal compositions (at.%) Nb-24Ti-16Si-5Cr-7B, Nb-24Ti-16Si-5Al-7B, Nb-24Ti-18Si-5Al-5Cr-8B and Nb-24Ti-17Si-3.5Al-5Cr-6B-2Mo, respectively. The alloys made it possible to compare the effect of B addition on density, hardness or oxidation with that of Ge or Sn addition. The alloys were made using arc melting and their microstructures were characterised in the as cast and heat-treated conditions. The B macrosegregation was highest in TT8. The macrosegregation of Si or Ti increased with the addition of B and was lowest in TT8. The alloy TT8 had the lowest density of 6.41 g/cm3 and the highest specific strength at room temperature, which was also higher than that of RCCAs and RHEAs. The Nbss and T2 silicide were stable in the alloys TT2 and TT3, whereas in TT4 and TT8 the stable phases were the Nbss and the T2 and D88 silicides. Compared with the Ge or Sn addition in the same reference alloy, the B and Ge addition was the least and most effective at 800 °C (i.e., in the pest regime), when no other RM was present in the alloy. Like Ge or Sn, the B addition in TT2, TT3 and TT4 did not suppress scale spallation at 1200 °C. Only the alloy TT8 did not pest and its scales did not spall off at 800 and 1200 °C. The macrosegregation of Si and Ti, the chemical composition of Nbss and T2, the microhardness of Nbss and the hardness of alloys, and the oxidation of the alloys at 800 and 1200 °C were also viewed from the perspective of the alloy design methodology NICE and relationships with the alloy or phase parameters VEC, δ and Δχ. The trends of these parameters and the location of alloys and phases in parameter maps were found to be in agreement with NICE.

1. Introduction

Research is underway worldwide to develop new metallic ultra-high temperature materials (UHTMs) to replace Ni superalloys in the hottest parts of future aero-engines to enable the latter to meet environmental and performance targets. Candidate metallic UHTMs include refractory metal (RM) intermetallic composites (RMICs), RM high entropy alloys (RHEAs) and RM complex concentrated alloys (RCCAs) (unnecessarily, in our opinion, another term has been added for RHEAs and RCCAs to further muddle the names used for metallic UHTMs, namely refractory chemically complex alloy (RCCAs)). The new materials must meet specific property targets (goals) for toughness, creep and oxidation resistance [1]. RMICs include materials based on Nb (RM(Nb)ICs, also known as Nb silicide-based alloys or Nb in situ composites) and Mo (RM(Mo)ICs). Recently, RM(Nb)ICs, RHEAs and RCCAs were compared in [1]. Some RM(Nb)ICs with B addition are also RCCAs [2] (i.e., RM(Nb)ICs/RCCAs). This paper is about RM(Nb)ICs with B addition and Ti/Si > 1.3 [1].
According to the alloy design methodology NICE (Niobium Intermetallic Composite Elaboration) [3], the alloying behaviour of RM(Nb)ICs and their phases, namely bcc Nb solid solution(s), M5Si3 silicides (M = RM = Mo, Ta or W, or M=TM (transition metal) = Cr, Hf or Ti), C14–NbCr2 based Laves and A15-Nb3X (X = Al, Ge, Si or Sn) compounds can be described using the parameters ΔHmix, ΔSmix, δ, VEC, Δχ, Ω (=Tm ΔSmix/|ΔHmix|) that are also used to describe the alloying of HEAs (see Appendix A). RM(Nb)ICs and their phases, and HEAs can be presented in maps of the above parameters [4,5,6,7,8,9]. Solid solution(s) RHEAs and RCCAs, and multiphase RCCAs (bcc solid solution(s) + M5Si3 silicide with/without Laves phase) can be presented in maps of aforementioned parameters together with RM(Nb)ICs and their bcc solid solution(s) [1]. The RM(Nb)ICs with B addition occupy a separate distinct area in the maps [1,2,5].
Boron in RM(Nb)ICs partitions to the bcc solid solution, the 5-3 silicide [4,6,10,11] and Nb3Si [11,12]. According to the Nb–Si–B phase equilibria, the 5-3 silicides are (a) the tetragonal T2 with Cr5B3 prototype, the same as D8l αNb5Si3, where B substitutes Si and becomes Nb5(Si,B)3, and (b) the hexagonal silicide with Mn5Si3 prototype, which is the same for the D88 γNb5Si3, i.e., the metastable 5-3 silicide in the Nb–Si binary [13], and the D88 Ti5Si3 [14], and in which B occupies the interstitial site of Si and the silicide becomes Nb5Si3Bx [10]. The latter is referred to as the D88 silicide.
According to the 1600 °C isothermal section of Nb–Si–B by Nowotny et al. [10], the B and Si concentrations in the T2 and D88 silicides are in the ranges (at.%) 5.5 < B < 21 and 17 < Si < 33, and 5 < B < 16 and 27 < Si < 37.5, respectively, the T2 and D88 have homogeneity range along the direction parallel to the Si-B binary [10,15] and a composition variation (≤2.5 and 5.5 at.%, respectively) along the direction parallel to the Nb–Si binary [10] and the Nb content of the D88 is in the range 54 < Nb < 60. The D88 has Si + B ≤ 42.5 at.% whereas the T2 has Si + B around 38 at.%. At 1600 °C, Sun et al. [11] calculated the maximum solubility of B in T2 to be 23.5 at.%, the B concentration in D88 in the range 10 < B < 15 at.% along the Si–B direction and the Nb concentration in D88 to be 55.6 ± 1 at.%. The latter is in good agreement with the average of 57 at.% [10] and gives Nb/(Si + B) about 1.3 in D88 compared with 1.7 for the T2. The B solubility in the D88 decreases with increasing temperature [15].
In this paper, we study the microstructure and properties of four RM(Nb)ICs based on Nb-24Ti-xSi-yB with additions of Al, Cr or Mo (x = 16, 17 or 18, y = 6, 7 or 8) that were selected so that they belong in area C in the Δχ versus δ, ΔHmix versus Δχ, ΔHmix versus VEC or VEC versus δ maps in [1,2,5]. The nominal composition of each alloy (at.%) was Nb-24Ti-16Si-5Cr-7B (alloy TT2), Nb-24Ti-16Si-5Al-7B (TT3), Nb-24Ti-18Si-5Al-5Cr-8B (TT4) and Nb-24Ti-17Si-3.5Al-5Cr-6B-2Mo (TT8), respectively (Table 1). These alloys are essentially based on specific KZ series alloys to which B has been added. In other words, the basis or reference alloys for TT2, TT3, TT4 and TT8, respectively are the alloys KZ4, KZ7, KZ5 [16] and JG3 [17] (for the nominal compositions of the reference alloys see Table A1 in Appendix A). Relevant data for the reference alloys are used to study how the addition of B in each alloy of this study affected microstructure and properties.
The structure of the paper is as follows: the description of experimental procedures is followed by the presentation of the results for the microstructures, density and hardness of the alloys. Preliminary results of the oxidation of the alloys are presented to show the effect of the addition of B on oxidation at 800 and 1200 °C. The discussion of the results includes their scrutiny from the perspective of NICE.

2. Experimental Section

Large button ingots (0.6 kg) of the alloys (Table 1) were prepared from high purity (min. 99.99 wt.%) Al, Cr, Mo, Nb, Si, Ti and B (99.5 wt.%) in an argon atmosphere using arc melting with a non-consumable tungsten electrode and a water-cooled copper crucible. Each alloy was melted five times. The alloys were heat-treated for 100 h at 1500 °C (1200 °C for TT2, see next section). Each alloy was wrapped in Ta foil and was heat-treated in a tube furnace under a continuous flow of Ti gettered argon followed by furnace cooling to room temperature. The microstructures of the alloys were characterised with XRD (Philips diffractometer, Hiltonbrooks Ltd., Crewe, UK, Cu radiation, solid specimens, JCPDS database) and microanalysis using EPMA (JEOL 8600 electron probe micro analyser, Tokyo, Japan, operating conditions 9 kV with a beam current of 30 nA [18]) equipped with WDX and EDX spectrometers, elemental standards and BN and TiN standards. The samples were prepared following standard metallographic procedures, mounted in Bakelite and ground using SiC grinding papers (320 to 2400 grit) and polishing with diamond DUR clothes (6 and 1 μm finish).
The density of the alloys was measured using Archimedes principle and a Sartorious electronic precision balance, Sartorius Lab Instruments GmbH & Co. KG, Göttingen, Germany, equipped with a density measurement kit. The isothermal oxidation of the as cast (AC) alloys was studied at 800 and 1200 °C using Stanton Redcroft thermo-balances (Thermal Scientific plc., Odessa, TX, USA) and specimens from the as cast alloys. The weight of each sample was measured at the start and end of each oxidation experiment. A Mitutoyo HM-101 hardness testing machine (Mitutoyo America, Aurora, IL, USA) with Vickers indenter was used to measure the hardness (0.5 kg load) of the as cast (AC) and heat-treated (HT) alloys. The microhardness of the solid solution and T2 silicide was measured in the AC and HT alloys using a 0.025 kg load. At least ten measurements were done for each alloy and condition, and each phase. The area fraction of the solid solution was measured using the software KS Run 3 in a Polyvar Met microscope. The SEM images of the large areas (×250) of the as cast (AC) and heat-treated (HT) alloys that were analysed by EPMA were used for the measurements.

3. Results

The actual composition of each alloy in the AC or HT condition is given in Table 1. The densities of the alloys are given in Table 2. The alloys TT4 and TT2 had the lowest and highest density, respectively, and the densities of all four alloys were lower than 7 g/cm3. The macrosegregation of solutes (MACX, X = Al, B, Cr, Si, Ti) in the alloys is given in Table 3. Note that this table has data for the Al and Cr free alloy TT1, to help us understand the role of boron with other alloying additions on MACX. The highest macrosegregation of B and Si was observed respectively in the alloys TT8 and TT4 whereas the macrosegregation of Ti was essentially similar in all four alloys. The phases that were observed in the alloys using XRD and EPMA are summarised in Table 4. The chemical compositions of the phases that were observed in all parts of the ingots are given in Table 5.

3.1. As Cast Alloys

In all parts of the ingot of the alloy TT2, were observed the Nbss, T2, a Cr and Ti-rich phase and a eutectic of the Nbss and T2, whereas in specific parts of the ingot other phases were also present, namely a Ti-rich phase in the top and bottom, a C14-Laves phase in the top and bulk and Nb3Si silicide in the bulk (Table 4 and Table 5, Figure 1a and Figure S1a in Supplementary Materials). Ti-rich Nbss and Ti-rich T2 were also observed. In Figure 1a, the grey contrast facetted phase is the T2, the bright contrast phase is the Nbss, darker contrast areas at the edges of Nbss are Ti-rich Nbss and darker grey contrast areas in between Nbss are Ti-rich T2. The Ti-rich phase, C14-Laves phase, Cr and Ti-rich phase and Nb3Si were observed in the dark and very contrast inter-dendritic Nbss areas. The average compositions of the Ti-rich phase, the Laves phase and the Nb3Si silicide, respectively, were 23.2(18.6–27.9)Nb-52.3(47.8–56.7)Ti-8.9(8.4–9.4)Si-14.7(14–15.5)Cr-0.9(0.8–1)B, 13.4(12.6–14.1)Nb-31.6(27.5–34.2)Ti-7.8(6.7–9)Si-47.7(45.3–49)Cr and 25.9(21.7–29)Nb-42.4(43–44.1)Ti-23.4(19.4–26.5)Si-7.9(4–11.3)Cr, where in the parentheses are given the minimum and maximum analysis values for each phase. It should be noted that the Laves and Nb3Si compounds were B free and that the Si concentration in the silicide would suggest also the presence of metastable Nb3Si [11], which however was not indicated by the XRD (Figure S1a in Supplementary Materials). In the Nbss, with increasing Ti concentration, the concentrations of B and Cr respectively decreased and increased, whereas in the T2 the B concentration decreased with increasing Ti concentration (Table 5). The average <Si> content and the <Nb>/<Si> and Si/B ratios of the T2 and Ti-rich T2 were 38.2 and 37.1 at.%, 1.6 and 1.7, and 2 and 3.8, respectively (where <Nb> = Nb + Cr + Ti and <Si> = B + Si). The T2 silicide was facetted, this was particularly noticeable in the top and bottom of the ingot. The vol.% of the eutectic was lower in the bulk.
In all parts of the ingot, the microstructure of the alloy TT3 consisted of the Nbss, T2, and eutectic of these two phases (Table 4 and Table 5, Figure 1c and Figure S1c in Supplementary Materials). The XRD suggested the presence of the D88 silicide, however, its presence was not confirmed by EPMA. Ti-rich Nbss and T2 were also observed but in this alloy the partitioning of Ti to T2 was very strong and resulted in distinct separate T2 grains very rich in Ti (and Al) in the top and bulk of the ingot, with average composition 34.2(29.8–37.2)Nb-28.2(24.7–32.2)Ti-27.8(26.6–28.8)Si-4.2(3.7–4.9)Al-5.6(3.6–7.4)B. In Figure 1c, the light contrast phase is the Nbss, the grey contrast phase is the T2 and the darker grey contrast is the Ti-rich T2. In the Nbss and T2, with increasing Ti concentration, the concentrations of both B and Al decreased in the solid solution, and respectively decreased and increased in the T2. The average <Si> content, and the <Nb>/<Si> and Si/B ratios of the T2, Ti-rich T2 and T2 very rich in Ti were 38.6, 39 and 37.5 at.%, 1.6, 1.56 and 1.67, and 1.9, 4 and 5, respectively (where <Nb> = Nb + Ti and <Si> = Al + B + Si). The T2 was facetted only in the bulk of the ingot. Cracks that had formed in large Ti-rich T2 grains were stopped by the surrounding solid solution.
In all parts of the ingot of the alloy TT4, the Nbss, T2, D88 and eutectic of Nbss and T2 were observed. The D88 silicide exhibited very bright contrast (Table 4 and Table 5, Figure 1e and Figure S1e in Supplementary Materials). Ti-rich Nbss and Ti-rich T2 were also observed but there was no evidence of Ti-rich D88. The latter was Al free. In Figure 1e, the T2 is the grey contrast phase, darker grey contrast areas correspond to Ti-rich T2, the very bright contrast phase with no darker contrast areas is the D88 (e.g., the very bright contrast thin long phase at the bottom left-hand side, middle and upper right-hand side of the image “running” at about 45 degrees from right to left) and the bright phase is the Nbss with darker areas corresponding to the Ti-rich Nbss.
In the Nbss and T2, with increasing Ti concentration, the concentrations of B and Cr decreased and increased, respectively, and the concentration of Al essentially did not change in the solid solution, whereas in the T2 the Al and Cr increased and the B decreased. The average <Si> content, and the <Nb>/<Si> and Si/B ratios of the T2, Ti-rich T2 and D88 were 38.2, 36.7 and 40.8 at.%, 1.62, 1.72 and 1.45, and 4.3, 6.4 and 0.6, respectively (where <Nb> = Nb + Ti + Cr and <Si> = Al + B + Si). The T2 was facetted in the top and the bulk of the ingot and Ti-rich T2 grains were cracked with the cracks parallel to each other and not extending in the surrounding Nbss.
The microstructure of the alloy TT8 consisted of Nbss, T2, D88, Nbss + T2 eutectic in all parts of the ingot and Nb3Si that was observed only in the top and bulk of the ingot (Table 4 and Table 5, Figure 1g and Figure S1g in Supplementary Materials). The average composition of Nb3Si was 46Nb-23Ti-20.1Si-2.8Al-10Cr-5.8B-1.3Mo. The D88 exhibited very bright contrast and was Al free. In Figure 1g, the T2 is the grey contrast phase, darker grey contrast areas correspond to Ti-rich T2, the very bright contrast phase with no darker contrast areas around it is the D88, and the bright phase with darker areas is the Nbss. The Nb3Si exhibits very dark contrast in the inter-dendritic Nbss areas. The concentration of B in the solid solution varied significantly. It should be noted that there were solid solution grains that were B free. Ti-rich Nbss and Ti-rich T2 were also observed, and no Ti-rich D88. In the Nbss and T2, with increasing Ti concentration, the concentrations of Al, B and Mo decreased and that of Cr increased in the solid solution whereas in the T2 the B decreased but the changes of Al, Cr and Mo were minimal. The average <Si> content, and the <Nb>/<Si> and Si/B ratios of the T2, Ti-rich T2 and D88 were 38.9, 37.7 and 42.6 at.%, 1.57, 1.65 and 1.35, and 2.5, 3.3 and 0.4, respectively (where <Nb> = Nb + Ti + Cr and <Si> = Al + B + Si). Both the T2 and D88 were facetted, particularly the latter and there were cracks in T2 that run parallel to each other and stopped at the Nbss.
The vol.% of the Nbss was essentially the same in the alloys TT2, TT3 and TT8, about 38% and significantly lower in the alloy TT4 (Table 2). The microhardness of the solid solution was lowest and highest respectively in the alloys TT2 and TT4 (472 and 563 HV, respectively), the microhardness of T2 was highest and lowest in the alloys TT2 and TT3, respectively (1346 and 1232 HV, respectively), and the highest and lowest alloy hardness was measured for the alloys TT8 and TT3, respectively (744 and 630 HV, respectively), see Table 2.

3.2. Heat Treated Alloys

All the alloys were heat-treated at 1500 °C with the exception of the alloy TT2 that exhibited liquation at this temperature and was heat-treated at 1200 °C. The phases that were present in their microstructures are given in Table 4. The alloys TT2 and TT8 were contaminated by nitrogen during the heat treatment.
In the alloy TT2 the Nb3Si silicide, the Ti-rich phase, the Cr and Ti-rich phase and the Laves phase that were present in the cast alloy were not observed. The Nbss and T2 were present with Ti-rich areas in the latter (Table 4 and Table 5, Figure 1b and Figure S1b in Supplementary Materials). In Figure 1b, the light contrast areas are the Nbss, the grey contrast phase is the T2, the darker grey contrast is the Ti-rich T2 and the very dark areas are TiN. The chemical inhomogeneity that was characteristic of this alloy in the as cast condition resulted in T2 grains in the heat-treated microstructure with <Nb>/<Si> and Si/B ratios covering a wider range than in the other alloys. The chemical composition of T2 and Ti-rich T2 did not change significantly compared with the cast alloy (Table 5), the former had <Si> = 37.2 at.% (<Nb>/<Si> = 1.69) and Si/B about 1.9 whereas the latter had Si + B in the range 34.1 to 37 at.% (or <Nb>/<Si> in the range 1.7 to 1.93) and Si/B about one. The average composition of the Ti-rich T2 was as follows in different parts of the heat-treated ingot: in the top 39.9(37.7–42.4)Nb-20.8(17.4–24.1)Ti-18.6(17.1–19.6)Si-2.2(1.8–2.9)Cr-18.5(16.7–20.2)B, in the bulk 42.4(41.4–43.9)Nb-20.6(19.4–21.2)Ti-19.7(18.4–21.4)Si-2.2(1.7–2.7)Cr-15.2(13.3–17.6)B, and in the bottom (where only one analysis was possible) 41.5Nb-19.2Ti-18.1Si-2.4Cr-18.9B. In the bottom of the heat-treated alloy there were also areas of the Ti-rich T2 where the Si and B concentrations were not equal, with <Si> = 37 at.% (<Nb>/<Si> = 1.7) and Si/B about 3.8 (41.7(39.6–43.5)Nb-20.8(18.4–22.4)Ti-29.3(27.9–30.3)Si-7.7(6.5–9.8)B-0.5(0.4–0.7)Cr). Furthermore, there were Ti-rich T2 grains with <Si> = 35.1 at.% (<Nb>/<Si> = 1.85) and Si/B = 6.3 (where <Si> = Si +B, <Nb> = Nb + Cr + Ti).
The microstructures of the alloys TT3 and TT4 consisted of the Nbss, T2 with the D88 present only in the latter alloy and no TiN in both alloys. Ti-rich T2 was observed in TT3 but not in TT4 and the D88 was Al free, as was the case in the cast alloy (Table 4 and Table 5, Figure 1d,f and Figure S1d,f in Supplementary Materials). The microstructure of TT3-HT is shown in Figure 1d, where the light contrast phase is the Nbss, the grey contrast phase is the T2 and the darker grey contrast is the Ti-rich T2. In the alloy TT3, the average <Si> content, and the <Nb>/<Si> and Si/B ratios of the T2 and Ti-rich T2 were 38.5 and 37.7 at.%, 1.6 and 1.65, and 2.6 and 6.1, respectively (where <Nb> = Nb + Ti and <Si> = Al + B + Si). In the TT4-HT there were no facetted T2 grains and often the D88 silicide was observed inside (surrounded by) T2 grains. The microstructure of TT4-HT is shown in Figure 1f, where the bright phase is the Nbss, the grey phase is the D88 and the darker grey contrast phase is the T2. The T2 had <Si> = 39 at.%, <Nb>/<Si> = 1.56, Si/B = 5.5 (<Si> = Al + B + Si, <Nb> = Nb + Cr + Ti), whereas the D88 had <Si> = 42.7 at.%, <Nb>/<Si> = 1.3 and Si/B = 0.5. In the alloy TT8 the microstructure consisted of Nbss, the T2, D88 and Ti-rich T2 silicides, was contaminated by nitrogen and the Nb3Si was not present (Table 4 and Table 5, Figure 1h and Figure S1h in Supplementary Materials). The D88 was Al free. The microstructure of TT8-HT is shown in Figure 1h, where the bright phase is the Nbss, the grey phase is the D88, the darker grey contrast phase is the T2 and dark areas around the latter correspond to Ti-rich T2. The average <Si> content, and the <Nb>/<Si> and Si/B ratios of the T2, Ti-rich T2 and D88 were 37.3, 38.3 and 40 at.%, 1.68, 1.61 and 1.5, and 6.2, 4.1 and 0.51, respectively (<Nb> = Nb + Cr + Mo + Ti). Some grains for the Nbss were B free, as in TT8-AC.
After the heat treatment, the vol.% of Nbss increased slightly in the alloys TT2, TT3 and TT8 and significantly in TT4 and was similar in all alloys, about 39% (Table 2). The microhardness of the Nbss was reduced in all alloys, most noticeably in TT3. Similarly, the microhardness of T2 was reduced in all alloys, but the smallest reduction was in TT4. The hardness of all alloys was reduced, the TT8 still had the highest hardness but the smallest hardness reduction was measured for TT2 (Table 2).

3.3. Oxidation

The mass change data is shown in Figure 2a,b for isothermal oxidation at 800 and 1200 °C and typical examples of scale spallation at the two temperatures are shown in Figure 2c,d. The Figure 2a,b include data for the MASC alloy (Nb-25Ti-16Si-2Al-2Cr-8Hf [20]) and the alloy TT1 [12]. The oxidation rate constants are given in Table 6. At 800 and 1200 °C, all four alloys followed respectively linear and parabolic oxidation kinetics. None of the alloys with B addition suffered from pest oxidation at 800 °C, meaning each alloy did not convert into powder, but the scales that formed on the alloys TT1, TT2, TT3 and TT4 spalled off. At 1200 °C scale spallation was also observed for the alloys TT1, TT2, TT3 and TT4, and the MASC alloy. The 1200 °C specimen of TT8 looked exactly like the specimen shown in Figure 2d.

4. Discussion

4.1. Macrosegregation

The addition of B increased the macrosegregation of Ti and Si compared with the reference B free alloys, with the exception of TT8 where MACSi decreased compared with JG3 (Table 7). TT4 had the highest MACSi, an increase of 3.4 at.% compared with KZ5, and TT1 had the highest MACTi. The highest and lowest MACB was exhibited respectively by TT8 and TT4. With the exception of the alloy TT4, the spread of MACB was narrow and around 4.4 at.%.
The macrosegregation of Si and Ti in the alloys of this study and their reference alloys is shown in Figure 3a–p. This figure shows plots of MACSi and MACTi versus specific parameters that describe macrosegregation in RM(Nb)ICs [19]. In agreement with previous research on B free RM(Nb)ICs [21,22,23,24], RM(Nb)ICs/RCCAs [25] and HEAs [26] both MACSi and MACTi increased with ΔHmsp, ΔHm/Tm, [ΔHm/Tm] × [ΔHmsd/ΔHmsp]−1 and Tmsp, and decreased with ΔHmsd, ΔHmsd/ΔHmsp, Tmsd and Tmsd/Tmsp (for definitions and equations for above parameters, please refer to [19]). This means that alloy design in NICE can optimise both MACSi and MACTi in B containing alloys using the same parameters. It should be noted that in the MACSi plots the data for the alloy TT8 and its basis JG3 does not follow the aforementioned trend. Further research is essential to confirm MACSi in TT8 and to study RC(Nb)ICs based on TT4 with RM addition(s) as both alloys (i.e., TT4 and TT8) point to a “pathway” for developing RCCAs with B addition [1,2].
The data for MACB is limited only to the alloys of this study and the alloy TT1 [12]. Figure 3q to s show a good parabolic fit of this limited data of MACB versus the parameters ΔHmsd, ΔHmsd/ΔHmsp and Tmsd, and suggests “maximum” MACB between five and six at.% for ΔHmsd ≈ 18 kJ/mol, ΔHmsd ≈ 1.535 kJ/mol and Tmsd ≈ 1840 K. More data about MACB is needed before we can firmly ascertain that the same parameters and trends also describe the macrosegregation of B in RM(Nb)ICs, and RHEAs or RCCAs with B addition.

4.2. Microstructures

The alloy microstructures were chemically inhomogeneous, particularly in the case of the alloy TT2. In the reference alloys KZ7, KZ5 and JG3, the high-temperature tetragonal βNb5Si3 had formed from the melt [16,17], whereas with the addition of B, in the alloys TT2, TT3, TT4 and TT8 the tetragonal T2 silicide (same structure as the low-temperature αNb5Si3, see introduction) formed from the melt as did the hexagonal D88 silicide in the alloys TT4 and TT8. In the reference alloy KZ4, the αNb5Si3 formed via the eutectoid transformation of Nb3Si [16]. Solute partitioning made the identification of phases, in particular the D88 silicide in the alloys TT4 and TT8, difficult. In all four alloys, the Nbss and T2 were stable phases and the D88 in TT4 and TT8.
In the alloy TT2 the Ti-rich phase, Nb3Si and C14 Laves phase formed in competition with the Cr and Ti-rich phase (Table 4) in specific parts of the ingot of the cast alloy. The Ti-rich phase was observed only in the top and bottom of the ingot, the Laves phase in the top and bulk, similarly to KZ4-AC [16], and the Nb3Si silicide only in the bulk. The aforementioned four phases were not stable in the heat-treated alloy. Note that the C14 Laves phase was also not stable in KZ4-HT. The Nbss + Nb3Si eutectic that formed in KZ4-AC was replaced by the Nbss + T2 eutectic in TT2-AC. In the latter, the area fraction of the eutectic was significantly reduced in the bulk of the ingot rather than at the bottom, which was the case in TT1-AC [12], and would suggest sensitivity of the Nbss + T2 eutectic to cooling rate and the presence or not of the Nb3Si silicide. The Laves phase formed from Cr rich melt and thus depended on the partitioning of Cr during solidification. This would explain why the Laves phase was not observed in the bottom of the ingot. Compared with KZ4-AC, no Ti-rich areas were observed in the Laves phase in TT2-AC and the Ti concentration was significantly higher than in the Laves phase in KZ4-AC. This was attributed to the Laves phase “competing for Ti” with the Cr and Ti-rich phase (which formed everywhere in the ingot) and the Ti-rich phase (which formed in the top and bottom of the ingot). Chemical inhomogeneity existed in TT2-HT, with a range of composition of the Ti-rich T2 (see Table A2 in the Appendix A) indicating that equilibrium was not reached in this alloy after 100 h at 1200 °C.
The as solidified microstructure in TT3 was similar to that in KZ7-AC [16], the Nbss + βNb5Si3 eutectic in the latter was replaced by the Nbss + T2 eutectic in TT3-AC. Compared with TT1-AC, the addition of Al in TT3 suppressed the formation of Nb3Si, which was also the case in KZ7-AC compared with KZ3-AC [16]. The suppression of the Nb3Si was also linked with the strong partitioning of Ti in the T2 that “starved” the melt of Ti, which stabilises the Nb3Si. Therefore, the synergy of B and Al in TT3 furthered the formation of primary tetragonal T2 (as did the addition of Al in KZ7 regarding the formation of primary βNb5Si3 [16]) and of the Nbss + T2 eutectic. The partitioning of Ti in T2 was sensitive to cooling rate as the very Ti-rich T2 was not observed in the bottom of the ingot of TT3-AC.
In the alloy TT4, the C14 Laves phase was not formed, differently with KZ5-AC [16]. In the alloy TT8-AC, the Nb3Si silicide was formed but not the C14 Laves, similarly with JG3-AC [17], in which Nbss + Nb3Si eutectic was formed compared with the Nbss + T2 eutectic in TT8-AC. The Nb3Si was not observed in the bottom of the ingot of TT8-AC. Comparison with the data for JG3-AC [17] and TT8-AC would suggest sensitivity of the formation of Nb3Si to cooling rate that was attributed to the synergy of B, Cr and Mo in which B and Cr lead. Three-phase equilibria between Nbss, Nb5Si3 and Nb4Si (metastable silicide) would exist for an alloy of composition Nb-17.5Si-2Mo (at.%) according to the ternary Nb-Si-Mo system by Savitskiym et al. [27]. The Nb3Si in TT8-AC had Si + B + Al ≈ 28.7 at.%, which is close to the composition of the metastable Nb3Si-m in [13], and the Si content (20.1 at.%) corresponds to Nb4Si (metastable silicide, [13]). Thus, it is likely that with the addition of Mo both the stable (i.e., tetragonal) and metastable Nb3Si silicide(s) formed in TT8-AC. Compared with JG3-AC, the Nb3Si was leaner in Si and Al and richer in Cr; this was attributed to the synergy of Mo and B in TT8. The concentration of Mo was the same in the Nb3Si in JG3-AC and TT8-AC, which would suggest that B did not affect the concentration of Mo in the 3-1 silicide. Compared with TT1-AC [12], the Nb3Si in TT8-AC was leaner in Si but richer in B. Compared with TT2-AC, the Nb3Si in TT8-AC was leaner in Si but richer in Cr and B. Given that in TT2-AC the Nb3Si was B free, it was concluded that in the presence of Mo the solubility of B in Nb3Si is increased and that Mo leads in the Mo and Cr synergy and eliminates the negative effect of Cr on the solubility of B in Nb3Si.
In both the TT4 and TT8 alloys (Ti/Si = 1.5 based on nominal compositions or average Ti/Si = 1.42 based on actual chemical compositions, Table 1), with the addition of B, a new B rich phase formed and was stable, namely the D88 silicide. The latter was observed in the areas surrounding the T2 and exhibited very strong bright contrast, which was stronger than that of Nbss (Figure 1e,g). There was no solubility of Al in D88 and its Ti concentration was in the range 10.2 < Ti < 12.5 at.% (average 11.7 at.%, Table 5). In all the alloys of this study, whether in the AC or HT condition, the Si + B or the Si + B + Al content of the T2 was essentially the same (37 and 38.1 at.%, respectively, average 37.6 at.%) whereas the Si + B content of the D88 was higher and in the range 40 to 42.7 at.% (average 41.5 at.%). Furthermore, the Si/B ratio in the T2 was in the range 1 to 6.4 (average 4) compared with 0.5 for the D88 silicide (range 0.4 to 0.6), and the average <Nb>/<Si> ratio was 1.7 in the T2 compared with 1.4 in the D88 (Table A2 in Appendix A). The Ti concentration of the T2 and D88, respectively, was in the ranges 14.3 to 30.7 at.% (average 21.2 at.%) and 10.2 to 12.5 at.% (average 11.7 at.%), Table 5. The above data for the T2 and D88 silicides is in agreement with the Nb-Si-B ternary [10], see introduction.
In the 1600 °C ternary Nb-Si-B section, tentative equilibrium between T2 and Nb3B2 was indicated by Nowotny et al. [10]. Thermodynamic modelling of the Nb–Si–B ternary [28] calculated the Nb3B2 to be stable at 1600 °C and showed that it formed two three-phase equilibria Nb + T2 + Nb3B2 and T2 + Nb3B2 + NbB with neighbouring phases. Sun et al. [28] stated “there are no direct experimental evidences to support the existence of these two three-phase equilibria” and “further experimental results are needed to accurately define the stability region of Nb3B2”.
The Nb3B2 compound was reported by the same researchers [11] in the B-rich, arc melted and heat-treated (1500 °C/100 h) very small buttons (0.006 kg) of seven Nb–Ti–Si–B alloys, of which six were B-rich (B ≥ 10 at.%) and one B-lean (B = 1.5 at.%), all alloys had 16 at.%Si, four had Ti/Si < 1 (range 0.28 to 0.9, Ti = 4.5, 6, 12, 14.5 at.%) and three had Ti/Si > 1 (range 1.1 to 1.47, Ti = 18, 20, 23.5 at.%). The microstructures of the alloys were studied using EPMA and XRD. One of their alloys, namely Nb-23.5Ti-16Si-10B, was close to the actual composition of the alloy TT1 [12] and its microstructure was reported to consist of Nbss, T2, Nb3Si and Nb3B2 compared with Nbss, T2 and Nb3Si for TT1. It should also be noted that the Nb3B2 compound was not reported in the microstructure of the Nb-22Ti-16Si-3Al-5Cr-4Hf-10B (at.%) alloy [29]. According to the EPMA data of Sun et al. [11], in the seven Nb-Ti-Si-B alloys that they studied, the Nb3B2 had 39.7 < Si + B < 42.2 at.% (average 41 at.%), 0.5 < Si/B < 0.76 (average 0.64), 1.9 < Ti < 11.4 at.% (average 6.2 at.%) and 1.37 < (Nb + Ti)/(Si + B) < 1.52 (average 1.44). The T2 silicide had 33.8 < Si + B < 38.9 at.% (average 37.2 at.%), 1 < Si/B <8.3 (average 3.5), 6.5 < Ti < 18 at.% (average 14 at.%) and 1.6 < (Nb + Ti)/(Si + B) < 2 (average 1.7). Differences for the Si/B ratio and Ti content in Nb3B2 and D88, and Ti content in T2, for the alloys studied by Sun et al. [11] and this work should be noted. In all four alloys of this work, the T2 was the primary phase. Considering the data for the alloy TT1 [12] and this work, there was two-phase Nbss and T2 equilibria in TT3, three-phase Nbss, T2 and Nb3Si equilibria in TT1 and three-phase Nbss, T2 and D88 equilibria in TT8. Only the synergy of B with Al and Al + Cr in the alloys TT3 and TT4 was able to control the contamination of the microstructure by nitrogen (Table 4).
The Si content in the Nbss increased with its Ti concentration (Figure 4a) and was essentially the same for all the HT alloys, about 0.5 at.%, the latter in agreement with other work on B-free RM(Nb)ICs e.g., [16,17]. Whereas the Si concentration was the same, the B content on the HT alloys varied depending on element(s) in synergy with B (Figure 4b). In the Ti-rich Nbss and “normal” Nbss the maximum B concentration respectively was about 6.1 and 3.2 at.%, which corresponded respectively to 1.7 and 1.9 at.%Si. The concentrations of B, Cr and Ti depended on each other, the Ti and B concentrations in the Nbss respectively increased and decreased with increasing Cr content in the Nbss (Figure 4c). As the Al + B + Ti content of the Nbss decreased the VEC of the solid solution increased, whereas the opposite was the case regarding B + Cr + Ti (Figure 4d). The VEC of the Nbss increases with Ti + Cr or Ti content in the alloys TT2, TT4 and TT8 (Figure 4e,f). The B or Mo content of the Nbss decreased with increasing Ti concentration in the Nbss (Table 5).
In the T2 silicide, the B content decreased and the Al and Cr concentrations increased as the Ti concentration increased ([6] and Table 5). Figure 5 shows maps of the T2 silicide in the AC and HT alloys TT2, TT3, TT4 and TT8 and of the Nb5Si3 silicide in the reference B-free alloys KZ4, KZ5, KZ7 and JG3. The T2 occupies a distinct, separate area in the Δχ versus VEC map (Figure 5a,b) in agreement with [2,6]. Both VEC and Δχ increase with increasing <Nb> and the linear fit of the data for T2 and Nb5Si3 is remarkably good (Figure 5c,d).

4.3. Hardness

The hardness of the Nbss decreased or increased with the parameter VECNbss when the alloys TT4 and TT8 were grouped respectively with the Cr containing alloy TT2 (Figure 6a) or the Al-containing alloy TT3 (Figure 6b). The same was the case for the reference alloys KZ5 and JG3 when grouped with the Cr or Al-containing alloys KZ4 and KZ7, respectively (Figure 6). The hardness of the Nbss in the AC and HT alloys TT2, TT4 and TT8 decreased with increasing VECNbss (Figure 6c).
The dependence of the hardness of the Nbss on solutes in the alloys is shown in Figure 7. The hardness decreased with increasing Ti + B + X or Ti + X content (X = Al, Cr), and this was linked with changes of the parameter VECNbss (Figure 4 and Figure 6), and also decreased with increasing Ti content in the Nbss, the same trend as for the reference alloys (Figure 7d). Note the link between Ti in the solid solution and its VEC (Figure 4f) and the change of hardness with VEC (Figure 6a).
The VECT2 or ΔχT2 increased with increasing <Nb> in T2 (Figure 5c,d) and the hardness of T2 increased with VECT2 (in [2]). The synergy of Cr with B and Ti decreased slightly the hardness of T2 in TT2-AC, which was the highest amongst the AC alloys of this study, compared with TT1-AC, but the T2 in TT2-HT did not retain its hardness after heat treatment, which decreased by 13% compared with 6% in TT1-HT ([12] and Table 2) and was essentially the same as the hardness of T2 in TT3-HT and the second-lowest amongst all the HT alloys (Table 2). Best hardness retention of the T2 and highest hardness after heat treatment was observed in the case of the alloy TT4. Compared with the alloys ZF4 [30], ZF5 [31] and ZF6 [32], which are similar respectively to TT2, TT3 and TT4 with the addition of Ge instead of B, the T2 had significantly lower hardness than Nb5Si3 in these three alloys. Compared with TT1, the T2 hardness in TT4-HT was not significantly different than that in TT1-HT [12], which was also lower than the Nb5Si3 in ZF3 [33]. It should be noted that the relationship between the hardness of T2 and VECT2 is opposite that of Nb5Si3 and VECNb5Si3 (in [2]).
Alloy hardness versus the parameters VECalloy, δalloy and Δχalloy is shown in Figure 8a–c. Room temperature specific strength calculated from hardness (σHV/ρ)alloy is shown in Figure 8d. The addition of B to the reference alloys caused a decrease in VECalloy and an increase in HValloy and (σHV/ρ)alloy. Notice that the B containing alloys occupy specific distinct areas in the HValloy versus δalloy or Δχalloy maps.
Furthermore, notice the location of the JG3 alloy in the HValloy versus Δχalloy map. The maximum specific strength of 385 MPa cm3g−1 for VECalloy = 4.45 from the parabola for B containing alloys in Figure 8d is significantly higher than those reported for RCCAs to date [1,2], and only slightly lower than that of the RM(Nb)ICs-RCCAs JZ4 and JZ5 [34].
The parameters VECalloy, δalloy and Δχalloy link with specific solutes and thus allow us (i) to link the hardness and specific strength of alloys with solute additions and; (ii) to use these relationships for the design of alloys using the alloy design methodology NICE [1,2,3]. We demonstrate such relationships for the alloys TT2, TT4 and TT8 and the solutes B, Cr and Ti in Figure 9.
The parameter VECalloy increased with (Ti + Cr)alloy (Figure 9a) whereas the parameters δalloy and Δχalloy decreased (Figure 9b,c). The shift towards higher HValloy with decreased VECalloy for the B-containing alloys (Figure 8a) was thus attributed to the lower (Ti + Cr) content in the alloys TT2, TT4 and TT8. The shift of the latter in separate distinct areas in the maps in Figure 8b,c was attributed to the increase of δalloy and Δχalloy with the decrease of (Ti + Cr)alloy (Figure 9b,c). The parameter VECalloy decreased and the δalloy and Δχalloy increased with increasing (Ti/Cr)alloy (Figure 9d,e,f). The alloys were separated in the VECalloy or δalloy versus (Ti/Cr)alloy maps, as was the case in the VECalloy or δalloy versus (Ti + Cr)alloy maps, but in the former two maps the case for Mo-containing alloys JG3 and TT8 was different, with VECalloy minimum at about 4.45 and δalloy maximum at about 15 for (Ti/Cr)alloy = 4.75. Note that VECalloy ≈ 4.45 corresponds to maximum HValloy and specific strength in Figure 8a,d. Similarly to the Δχalloy versus (Ti + Cr)alloy map, the alloys were not separated in the Δχalloy versus (Ti/Cr)alloy map (Figure 9c,f). Thus, even though there are relationships of the parameters VECalloy, δalloy and Δχalloy with (Ti + Cr)alloy, or (Ti/Cr)alloy, and the parameters VECalloy, δalloy and Δχalloy are used to design new alloys using NICE [1,2,3], only the parameter VECalloy links hardness or specific strength with specific solutes in NICE, (Ti + Cr)alloy and (Ti/Cr)alloy in the case demonstrated above. Furthermore, the parameters VECalloy, δalloy and Δχalloy also link with the (Ti + Cr + B) content of the alloys TT2, TT4 and TT8, as shown in the maps in Figure 9g,h,i. VECalloy is maximum for (Ti + Cr + B)alloy = 35.5 at.%. The HValloy versus (Ti + Cr + B)alloy map (not shown) shows minimum (685 HValloy) and maximum (740 HValloy) hardness, respectively, for AC and HT alloys for Ti + Cr + B = 35.5 at.% whereas the HValloy versus (Ti + Al + B)alloy map (not shown) shows minima of 615 HValloy and 560 HValloy with (Ti + Al + B)alloy equal to 34.5 and 35.5 at.%, respectively, for the AC and HT alloys TT3, TT4 and TT8. It should be noted that also the hardness of the solid solution (HVNbss) links with VECNbss (Figure 6) and with solutes, namely Ti + X, Ti + B + X (X = Al, Cr), and Ti/Cr (Figure 7) and that solutes in the Nbss link with its parameters (see Figure 4 for relationships with VECNbss for B containing alloys and Figure A1 in the Appendix A for relationships in the reference alloys). Such relationships allow the design methodology NICE to optimise alloy composition for the balance of strength and oxidation properties, see [1,2,3].
Figure 10 compares the density of the base alloys KZ4, KZ7 and KZ5 with that of the equivalent alloys with Ge addition, namely ZF4, ZF5 and ZF6 [30,31,32], and with B addition.
It is clear that the B addition had the most significant effect on reducing alloy density. Figure 11 compares the room temperature hardness of AC and HT alloys ZF4, ZF5, ZF6 [30,31,32] and TT2, TT3 and TT4. The addition of Ge to the reference alloys increased the alloy hardness compared with the addition of B. This was attributed (i) to the increase of the hardness of the Nb5Si3 when alloyed with Ge; and (ii) to the lower vol.% of Nbss in the Ge containing alloys [6,30,31,32] compared with the alloys TT2, TT3 and TT4.

4.4. Oxidation

The data for the alloys TT1, TT2, TT3, TT4 and TT8 can help us to infer what the effect of B addition to the reference alloys was on isothermal oxidation at 800 and 1200 °C and to compare the effect of B addition with that of Ge or Sn to the same reference alloys. Amongst the reference alloys KZ4, KZ5, KZ7 and JG3, the alloy JG3-AC had the best oxidation behaviour at both temperatures, did not pest at 800 °C, and followed parabolic oxidation at 800 °C and liner oxidation at 1200 °C (the JG3-HT followed linear oxidation at both temperatures) [35]. The rate constant of the alloys TT1, TT2 and TT3 at 800 °C (Table 6) was one order of magnitude higher than that of JG3-HT, and of the alloys TT4 and TT8 similar or one order of magnitude lower, respectively. The alloys KZ4, KZ5 and KZ7 formed Maltese crosses at 800 °C [36], like the MASC alloy, and their scales spalled off at 1200 °C, as did the scale of JG3.
At 800 °C, the mass change of TT1 was significantly lower than that of KZ3, which gained more than about 200 mg/cm2 after just 10 h. The synergy of B and Cr decreased the mass change compared with KZ4 (about 60 mg/cm2 after 100 h). The Al addition in TT3 also improved the oxidation behaviour compared with TT1 (Table 6). Compared with KZ7, the synergy of Al with B was only marginally beneficial for the first 20 h, after this time the mass change increased. The mass of the alloy TT4 did not change for the first 10 h and after this time it was lower than that of KZ5, which gained about 32.5 mg/cm2. The Mo addition in TT8 significantly improved the oxidation behaviour compared with JG3, which gained about 3.5 mg/cm2.
At 1200 °C, the synergy of Al and Cr in TT4 had a strong effect on oxidation behaviour (mass change after 90 h: TT1 = 80.3, TT2 = 105.6, TT3 = 66.1 and TT4 = 34.0 mg/cm2). The addition of Mo in the TT8 alloy resulted in a marginal improvement of the oxidation behaviour of TT8 compared with TT4. Figure 12 compares the mass changes of the alloys of this study with their reference alloys after 90 h at 800 or 1200 °C. In each part of this figure, the effect of B addition is indicated by an arrow. With the exception of TT3, whose mass increased more than KZ7 at 800 °C (Figure 12b), the addition of B resulted to lower mass changes at both temperatures, particularly in the case of the alloy TT8.
Plots of the mass changes of the B-containing alloys and their reference alloys versus the alloy parameters VEC and δ are shown in Figure 13. According to the alloy design methodology NICE, for improved oxidation behaviour, the alloy design should aim to lower VECalloy and increase δalloy [1,2,3]. Figure 13 shows that this was the case for all alloys at 1200 °C, and also at 800 °C where the alloy TT3 was the exception as its mass change was higher than that of KZ7 (Figure 12b and Figure 13a,b).
Compared with the Ge containing alloys ZF4, ZF5 and ZF6 [37] and the Sn containing alloys ZX4, ZX6 and ZX8 [22] (for nominal compositions see Table A1 in the Appendix A), the oxidation of the B-containing alloys TT2, TT3 and TT4 was inferior at 800 °C. Indeed, the above ZF and ZX series alloys did not pest, their scales did not spall off, and followed parabolic oxidation kinetics [37], or parabolic with/without linear kinetics [22]. At 1200 °C the ZF and ZX series alloys followed either parabolic plus linear kinetics [37] or parabolic or linear kinetics [22] and their scales spalled off, the same as the KZ series reference alloys. Only the alloy TT8 did not pest at 800 °C and its scale did not spall off at 800 and 1200 °C.
At 800 °C, the scales that formed on the alloys TT1 and TT2 consisted of SiO2, TiO2, Nb2O5, 3Nb2O5.TiO2, and 5Nb2O5.2TiO2, which are typical oxides in the scales of RM(Nb)ICs [3,35,36], plus B2O3 and B2SiO5 in TT1 plus CrNbO4 in TT2 (Figure S2a in Supplemental data). The scales that formed on TT3 and TT4 consisted of the same oxides as TT1, plus AlNbO4 in TT3 and CrNbO4 and AlNbO4 in TT4 (data not shown). At 1200 °C, the scale on TT1 consisted of SiO2, TiO2, Nb2O5 and 3Nb2O5.TiO2, 5Nb2O5.2TiO2, plus B2O3 and B2SiO5 whereas the scale on TT2 consisted of the same oxides plus NbO, and CrNbO4 (Figure S2b in Supplementary Materials). The scale of TT3 consisted of the same oxides as TT1 plus AlNbO4 (data not shown). The presence of CrNbO4 and AlNbO4 in the scales of the alloys TT2, TT3 or TT4 is in agreement with the data for the B free alloys KZ4, KZ7 and KZ5 [3,36] and the Ge containing alloys ZF4, ZF5 and ZF6, where also SiO2, Nb2O5, TiNb2O7 (Nb2O5.TiO2) and GeO2 were observed [37].
Comparison of the oxidation of the reference alloys KZ4, KZ7, KZ5 [36] with the alloys with B addition, namely TT2, TT3 and TT4, or Ge addition (ZF4, ZF5, ZF6 [37]) or Sn addition (ZX4, ZX6, ZX8 [22]) shows that at 800 °C (i.e., in pest regime) Ge and B, respectively, was most and least effective and that at 1200 °C all three elements were not effective as scale spallation was not suppressed. However, only when B was in synergy with Al, Cr and Mo was the oxidation improved compared with the basis alloy JG3 [35], as the alloy TT8 did not pest and its scale did not spall off at 800 and 1200 °C. Thus, the aforementioned synergy of elements in TT8 had the same effect at both temperatures as that of Al and Cr with Ge plus Sn in the alloy OHS1 [23]. In other words, the alloy TT8 had outstanding (for RMICs, and RHEAs and RCCAs) oxidation behaviour at 800 and 1200 °C with density 6.4 g/cm3 and specific strength of 377 and 337 MPacm3g−1, respectively, in AC and HT conditions. Another characteristic difference of the alloys with B or Ge addition [37] with the Sn containing alloys ZX4, ZX6 and ZX8 [22] was the fact that in the latter, tin oxide was rarely (if at all) observed in the scale, in contrast with the former alloys where B2O3 or GeO2 were formed. The latter two oxides form glass with silica.

5. Conclusions

We studied the effect of B addition on the density, macrosegregation, microstructure, hardness and oxidation of four RM(Nb)IC alloys, namely the alloys TT2, TT3, TT4 and TT8. In actual fact, these alloys were based on four KZ series alloys (the basis/reference alloys) to which B was added. This choice of alloys made it possible to also compare the effect of B addition on density, hardness or oxidation with that of Ge or Sn addition.
The addition of B resulted in B macrosegregation that was highest in TT8 and in increased macrosegregation of Si and Ti, both of which were lowest in TT8. With the B addition, the density of the alloys was decreased significantly and was lower than the alloys with Ge addition. The alloy TT8 had the lowest density of 6.41 g/cm3 and the highest specific strength at room temperature, which was also higher than that of RCCAs and RHEAs. The Nbss and T2 silicide were stable in the alloys TT2 and TT3, whereas in TT4 and TT8 the stable phases were the Nbss and the T2 and D88 silicides. The latter silicide was Al free. The T2 had Si + B + Al ≈ 37.5 at.%, Si/B ≈ 4 and <Nb>/<Si> ≈ 1.7 compared with Si + B ≈ 41.5 at.%, Si/B ≈ 0.5 and <Nb>/<Si> ≈ 1.4 of the D88. Compared with the Ge or Sn addition in the same reference alloy, the B and Ge addition was the least and most effective at 800 °C (i.e., in the pest regime), when no other RM was present in the alloy. Like Ge or Sn, the B addition in TT2, TT3 and TT4 did not suppress scale spallation at 1200 °C. Only the alloy TT8 did not pest and its scales did not spall off at 800 and 1200 °C.
The macrosegregation of Si and Ti, the chemical composition of Nbss and T2, the microhardness of Nbss and the hardness of alloys, and the oxidation of the alloys at 800 and 1200 °C were also viewed from the perspective of the alloy design methodology NICE and relationships with the alloy or phase parameters VEC, δ and Δχ. The trends of these parameters and the location of alloys and phases in parameter maps were found to be in agreement with NICE, the one exception being the macrosegregation of Si in TT8 when compared with its basis/reference alloy.

Supplementary Materials

The following are available online at https://0-www-mdpi-com.brum.beds.ac.uk/article/10.3390/ma14206101/s1, Figure S1: X-ray diffractograms (a), (c), (e) and (g) of AC alloys TT2, TT3, TT4 and TT8, respectively, and (b), (d), (e) and (h) of HT alloys TT2, TT3, TT4 and TT8, respectively; Figure S2: X-ray diffractograms of oxide scale formed on the alloy TT2 (a) at 800 °C and (b) at 1200 °C.

Author Contributions

Experimental work, T.T.; funding, P.T.; supervision, P.T.; formal analysis, T.T. and P.T.; draft preparation, T.T.; review, P.T., final paper, P.T. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the EPSC (EP/H500405/1, EP/L026678/1).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

All the data for this paper is given in the paper and its Supplementary Materials, other data cannot be made available to the public.

Acknowledgments

The support of this work by the University of Sheffield, Rolls-Royce Plc and EPSRC (EP/H500405/1, EP/L026678/1) is gratefully acknowledged.

Conflicts of Interest

The authors declare no conflict of interest.

Appendix A

δ = 100 n = 1 n c i   1 r i / r ¯ 2
Δ χ = n = 1 n c i   χ i   χ ¯ 2
V E C = n = 1 n c i   VEC i
r ¯ = n = 1 n c i   r i
χ   ¯ = n = 1 n c i   χ i
Δ H m i x = i = 1 , j 1 n Π i j   c i   c j  
Π i j = 4 Δ m i x A B
Δ S m i x = R i = 1 n c i   ln c i
T m = i = 1 n c i   T m i
where ci, ri, χi, (VEC)i and Tmi, respectively, are atomic percentage, atomic radius, Pauling electronegativity, VEC and melting point of ith element, Δ m i x A B   is the mixing enthalpy of binary liquid AB alloy and R is the gas constant.
Table A1. Nominal compositions (at.%) of reference alloys used in this work.
Table A1. Nominal compositions (at.%) of reference alloys used in this work.
Alloy Element
NbTiSiAlCrMoBGeSnRef.
JG3bal.2418552---[17]
KZ3bal.2418------[16]
KZ4bal.2418-5----[16]
KZ5bal.241855----[16]
KZ7bal.24185-----[16]
OHS1bal.241855--55[23]
TT1bal.2418---8--[12]
ZF3bal.2418----5-[33]
ZF4bal.2418-5--5-[30]
ZF5bal.24185---5-[31]
ZF6bal.241855--5-[32]
ZX4bal.2418-5---5[22]
ZX6bal.24185----5[22]
ZX8bal.241855---5[22]
Table A2. <Nb>/<Si> and Si/B ratios and Si + B and Si + B + Al sums in T2 and D88 silicides in AC and HT alloys, where <Nb> = Nb + TM + RM, <Si> = Al + B + Si, TM = Cr, Ti and RM = Mo.
Table A2. <Nb>/<Si> and Si/B ratios and Si + B and Si + B + Al sums in T2 and D88 silicides in AC and HT alloys, where <Nb> = Nb + TM + RM, <Si> = Al + B + Si, TM = Cr, Ti and RM = Mo.
Alloy and ConditionPhaseParameter
Si + B (at.%)Si/BSi + B + Al (at.%)<Nb/<Si>
TT2-ACT238.22-1.6
-Ti rich T237.13.8-1.7
TT2-HTT237.21.9-1.7
-Ti rich T2 *34.1 to 37
Average 35.6
1, 3.8, 6.3
Average 3.7
-1.7 to 1.9
Average 1.8
TT3-ACT2-1.938.61.6
-Ti rich T2-4391.56
-T2 very rich in Ti-537.51.67
TT3-HTT2-2.638.51.6
-Ti rich T2-6.137.71.65
TT4-ACT2-4.338.21.62
-Ti rich T2-6.436.71.72
-D8840.80.6-1.45
TT4-HTT2-5.5391.56
-D8842.70.5-1.3
TT8-ACT2-2.538.91.57
-Ti rich T2-3.337.71.65
-D8842.60.4-1.35
TT8-HTT2-6.237.31.68
-Ti rich T2-4.138.31.61
-D88400.5-1.5
* see text.
Figure A1. Data for the Nbss in HT boron free alloys KZ4, KZ5, KZ7 and JG3. (a)Ti + X (X = Al (blue), Cr (red)) versus the parameter Δχ for the alloys KZ4, KZ5, KZ7 and JG3, (b) and (c) Ti/Cr versus (b) δ for the alloys KZ4, KZ5 and JG3 and (c) Δχ for the alloys KZ7, KZ5 and JG3.
Figure A1. Data for the Nbss in HT boron free alloys KZ4, KZ5, KZ7 and JG3. (a)Ti + X (X = Al (blue), Cr (red)) versus the parameter Δχ for the alloys KZ4, KZ5, KZ7 and JG3, (b) and (c) Ti/Cr versus (b) δ for the alloys KZ4, KZ5 and JG3 and (c) Δχ for the alloys KZ7, KZ5 and JG3.
Materials 14 06101 g0a1

References

  1. Tsakiropoulos, P. Alloys for application at ultra-high temperatures: Nb-silicide in situ composites. Challenges, breakthroughs and opportunities. Prog. Mater. Sci. 2020, 123, 100714. [Google Scholar] [CrossRef]
  2. Tsakiropoulos, P. Refractory Metal (Nb) Intermetallic Composites, High Entropy Alloys, Complex Concentrated Alloys and the Alloy Design Methodology NICE—Mise-en-scène Patterns of Thought and Progress. Materials 2021, 14, 989. [Google Scholar] [CrossRef]
  3. Tsakiropoulos, P. On Nb Silicide Based Alloys: Alloy Design and Selection. Materials 2018, 11, 844. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  4. Tsakiropoulos, P. On the Nb silicide based alloys: Part I—The bcc Nb solid solution. J. Alloy. Compd. 2017, 708, 961–971. [Google Scholar] [CrossRef] [Green Version]
  5. Tsakiropoulos, P. On Nb silicide based alloys: Part II. J. Alloys Compd. 2018, 748, 569–576. [Google Scholar] [CrossRef] [Green Version]
  6. Tsakiropoulos, P. On the Alloying and Properties of Tetragonal Nb5Si3 in Nb-Silicide Based Alloys. Materials 2018, 11, 69. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  7. Tsakiropoulos, P. Alloying and Properties of C14–NbCr2 and A15–Nb3X (X = Al, Ge, Si, Sn) in Nb–Silicide-Based Alloys. Materials 2018, 11, 395. [Google Scholar] [CrossRef] [Green Version]
  8. Tsakiropoulos, P. Alloying and Hardness of Eutectics with Nbss and Nb5Si3 in Nb-silicide Based Alloys. Materials 2018, 11, 592. [Google Scholar] [CrossRef] [Green Version]
  9. Tsai, M.-H.; Yeh, J.-W. High-Entropy Alloys: A Critical Review. Mater. Res. Lett. 2014, 2, 107–123. [Google Scholar] [CrossRef]
  10. Nowotny, H.; Benesovky, F.; Rudy, E.; Wittmann, A. Aufban und Zunderverhalten von Niob-Bor-Silicium Legierungen. Monatch. Chem. 1960, 91, 975–990. [Google Scholar] [CrossRef]
  11. Sun, Z.; Yang, Y.; Guo, X.; Zhang, C.; Chang, Y.A. Austin Chang, Experimental investigation on the phase equilibria of the Nb-Ti-Si-B system at 1500 °C. J. Phase Equilibria Diffus. 2011, 32, 407–411. [Google Scholar] [CrossRef]
  12. Thandorn, T.; Tsakiropoulos, P. Study of the role of B addition on the microstructure of the Nb-24Ti-18Si-8B alloy. Intermetallics 2010, 18, 1033–1038. [Google Scholar] [CrossRef]
  13. Schlesinger, M.E.; Okamoto, H.; Gokhale, A.B.; Abbaschian, R. The Nb-Si (Niobium-Silicon) system. J. Phase Equilibria Diffus. 1993, 14, 502–509. [Google Scholar] [CrossRef]
  14. Okamoto, H. Phase Diagrams for Binary Alloys; Desk Handbook; ASM International: Metals Park, OH, USA, 2000. [Google Scholar]
  15. Katrych, S.; Grytsiv, A.; Bondar, A.; Rogl, P.; Velikanova, T.; Bohn, M. Structural materials: Metal-silicon-boron. The Nb rich corner of the Nb-Si-B system. J. Solid State Chem. 2004, 177, 493–497. [Google Scholar] [CrossRef]
  16. Zelenitsas, K.; Tsakiropoulos, P. Study of the role of Cr and Al additions in the microstructure of Nb-Ti-Si in situ composites. Intermetallics 2005, 13, 1079–1095. [Google Scholar] [CrossRef]
  17. Geng, J.; Tsakiropoulos, P.; Shao, G. The effects of Ti and Mo additions on the microstructure of Nb-silicide based in situ composites. Intermetallics 2006, 14, 227–235. [Google Scholar] [CrossRef]
  18. Yang, Y.; Chang, Y.; Tan, L.; Cao, W. Multiphase equilibria in the metal-rich region of the Mo–Ti–Si–B system: Thermodynamic prediction and experimental validation. Acta Mater. 2005, 53, 1711–1720. [Google Scholar] [CrossRef]
  19. Tsakiropoulos, P. On the macrosegregation of silicon in niobium silicide based alloys. Intermetallics 2014, 55, 95–101. [Google Scholar] [CrossRef]
  20. Bewlay, B.P.; Whiting, P.W.; Davis, A.W.; Briant, C.L. Creep Mechanisms in Niobium-Silicide Based In-Situ Composites. MRS Proc. 1998, 552, 6111. [Google Scholar] [CrossRef]
  21. Zacharis, E.; Utton, C.; Tsakiropoulos, P. A Study of the Effects of Hf and Sn on the Microstructure, Hardness and Oxidation of Nb-18Si Silicide Based Alloys without Ti Addition. Materials 2018, 11, 2447. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  22. Xu, Z.; Utton, C.; Tsakiropoulos, P. A Study of the Effect of 5 at.% Sn on the Micro-Structure and Isothermal Oxidation at 800 and 1200 °C of Nb-24Ti-18Si Based Alloys with Al and/or Cr Additions. Materials 2020, 13, 245. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  23. Hernández-Negrete, O.; Tsakiropoulos, P. On the Microstructure and Isothermal Oxidation at 800 and 1200 °C of the Nb-24Ti-18Si-5Al-5Cr-5Ge-5Sn (at.%) Silicide-Based Alloy. Materials 2020, 13, 722. [Google Scholar] [CrossRef] [Green Version]
  24. Zhao, J.; Utton, C.; Tsakiropoulos, P. On the Microstructure and Properties of Nb-12Ti-18Si-6Ta-2.5W-1Hf (at.%) Silicide-Based Alloys with Ge and Sn Additions. Materials 2020, 13, 1778. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  25. Zhao, J.; Utton, C.; Tsakiropoulos, P. On the Microstructure and Properties of Nb-12Ti-18Si-6Ta-5Al-5Cr-2.5W-1Hf Nb-Silicide Based Alloys with Ge and Sn Additions (at.%). Materials 2020, 13, 3719. [Google Scholar] [CrossRef] [PubMed]
  26. Ghadyani, M.; Utton, C.; Tsakiropoulos, P. Microstructures and Isothermal Oxidation of the Alumina Scale Forming Nb1.7Si2.4Ti2.4Al3Hf0.5 and Nb1.3Si2.4Ti2.4Al3.5Hf0.4 Alloys. Materials 2019, 12, 222. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  27. Savitskiy, E.M.; Baron, V.V.; Bychkova, M.I.; Bakuta, S.A.; Gladyshev, E.I.S. Phase diagram and properties of Nb- 795 Mo-Si alloys, Russian Metallurgy, Translated from Izvestiya Akademii Nauk SSSR. Metally 1965, 2, 91–96. [Google Scholar]
  28. Sun, Z.; Yang, Y.; Guo, X.; Zhang, C.; Chang, Y.A. Thermodynamic modelling of the Nb-rich corner in the Nb-Si-B system. Intermetallics 2011, 19, 26–34. [Google Scholar] [CrossRef]
  29. Zhang, S.; Guo, X. Effects of B addition on the microstructure and properties of Nb silicide based ultrahigh temperature alloys. Intermetallics 2015, 57, 83–92. [Google Scholar] [CrossRef]
  30. Li, Z.; Tsakiropoulos, P. Study of the effect of Cr and Ti additions in the microstructure of Nb–18Si–5Ge based in-situ composites. Intermetallics 2012, 26, 18–25. [Google Scholar] [CrossRef]
  31. Li, Z.; Tsakiropoulos, P. The microstructure of Nb-18Si-5Ge-5Al and Nb-24Ti-18Si-5Ge-5Al in situ composites. J. Alloy. Compd. 2013, 550, 553–560. [Google Scholar] [CrossRef]
  32. Li, Z.; Tsakiropoulos, P. On The Microstructures and Hardness of The Nb-24Ti-18Si-5Al-5Cr-5Ge and Nb-24Ti-18Si-5Al-5Cr-5Ge-5Hf (at.%) Silicide Based Alloys. Materials 2019, 12, 2655. [Google Scholar] [CrossRef] [Green Version]
  33. Li, Z.; Tsakiropoulos, P. Study of the effect of Ti and Ge in the microstructure of Nb-24Ti-18Si-5Ge in situ composite. Intermetallics 2011, 19, 1291–1297. [Google Scholar] [CrossRef]
  34. Zhao, J.; Utton, C.; Tsakiropoulos, P. On the Microstructure and Properties of Nb-18Si-6Mo-5Al-5Cr-2.5W-1Hf Nb-Silicide Based Alloys with Ge, Sn and Ti Additions (at.%). Materials 2020, 13, 4548. [Google Scholar] [CrossRef]
  35. Geng, J.; Tsakiropoulos, P.; Shao, G. Oxidation of Nb–Si–Cr–Al in situ composites with Mo, Ti and Hf additions. Mater. Sci. Eng. A 2006, 441, 26–38. [Google Scholar] [CrossRef]
  36. Zelenitsas, K.; Tsakiropoulos, P. Effect of Al, Cr and Ta additions on the oxidation behaviour of Nb–Ti–Si in situ composites at 800 °C. Mater. Sci. Eng. A 2006, 416, 269–280. [Google Scholar] [CrossRef]
  37. Li, Z.; Tsakiropoulos, P. The Effect of Ge Addition on the Oxidation of Nb-24Ti-18Si Silicide Based Alloys. Materials 2019, 12, 3120. [Google Scholar] [CrossRef] [PubMed] [Green Version]
Figure 1. Microstructures of the AC (a,c,e,g) and HT (b,d,f,h) alloys TT2 (a,b), TT3 (c,d), TT4 (e,f) and TT8 (g,h). Note that contrast enhancement has been applied to show different phases. For description of microstructures see text.
Figure 1. Microstructures of the AC (a,c,e,g) and HT (b,d,f,h) alloys TT2 (a,b), TT3 (c,d), TT4 (e,f) and TT8 (g,h). Note that contrast enhancement has been applied to show different phases. For description of microstructures see text.
Materials 14 06101 g001
Figure 2. Mass change (ΔW/A) versus time of alloys TT1, TT2, TT3, TTT4, TT8 and MASC at (a) 800 °C and (b) 1200 °C. Colours: black TT1, blue TT2, green TT3, red TT4, yellow MASC, brown TT8. Specimens of TT4 and TT8 after oxidation (c) at 1200 °C and (d) 800 °C, respectively.
Figure 2. Mass change (ΔW/A) versus time of alloys TT1, TT2, TT3, TTT4, TT8 and MASC at (a) 800 °C and (b) 1200 °C. Colours: black TT1, blue TT2, green TT3, red TT4, yellow MASC, brown TT8. Specimens of TT4 and TT8 after oxidation (c) at 1200 °C and (d) 800 °C, respectively.
Materials 14 06101 g002aMaterials 14 06101 g002b
Figure 3. MACSi (a,c,e,g,i,k,m,o), MACTi (b,d,f,h,j,l,n,p) and MACB (q,r,s) versus parameters for alloys TT1, TT2, TT3, TT4 and TT8, and their basis/reference alloys KZ3, KZ4, KZ5, KZ7 and JG3. Diamonds for B containing alloys. Colours (ap), brown TT1, KZ3, green TT2, KZ4, red TT3, KZ7, purple TT4, KZ5, blue TT8, JG3. Pink for the MACB data. The alloy TT8 is indicated in (q) to (s). If TT8 were to be excluded, the R2 values for the parabolic fit of the data change to 0.9986, 0.813 and 1, respectively in (q,r,s).
Figure 3. MACSi (a,c,e,g,i,k,m,o), MACTi (b,d,f,h,j,l,n,p) and MACB (q,r,s) versus parameters for alloys TT1, TT2, TT3, TT4 and TT8, and their basis/reference alloys KZ3, KZ4, KZ5, KZ7 and JG3. Diamonds for B containing alloys. Colours (ap), brown TT1, KZ3, green TT2, KZ4, red TT3, KZ7, purple TT4, KZ5, blue TT8, JG3. Pink for the MACB data. The alloy TT8 is indicated in (q) to (s). If TT8 were to be excluded, the R2 values for the parabolic fit of the data change to 0.9986, 0.813 and 1, respectively in (q,r,s).
Materials 14 06101 g003aMaterials 14 06101 g003bMaterials 14 06101 g003cMaterials 14 06101 g003dMaterials 14 06101 g003eMaterials 14 06101 g003fMaterials 14 06101 g003g
Figure 4. (a) Ti versus Si and (b) B versus Si content of the Nbss in the alloys TT1 [12], TT2, TT3, TT4 and TT8 where the data for HT alloys is shown in green. In (a) the R2 values are given for the linear or parabolic fit of data and in (b) the R2 values are for the parabolic fit of data, where blue filled circles correspond to Ti-rich Nbss and red to normal Nbss in AC alloy. (c) Element X versus Cr in Nbss, data for X = B (brown) or Ti (purple) in the Nbss of the HT alloys TT2, TT4 and TT8. (d) Ti + B + X (X = Al, Cr) versus VEC of Nbss in the HT alloys TT2, TT3, TT4 and TT8, purple X = Al, alloys TT3, TT4, TT8, pink X = Cr, alloys TT2, TT4, TT8, (e) Ti + Cr versus VEC and (f) Ti versus VEC of Nbss, HT alloys TT2, TT4, TT8.
Figure 4. (a) Ti versus Si and (b) B versus Si content of the Nbss in the alloys TT1 [12], TT2, TT3, TT4 and TT8 where the data for HT alloys is shown in green. In (a) the R2 values are given for the linear or parabolic fit of data and in (b) the R2 values are for the parabolic fit of data, where blue filled circles correspond to Ti-rich Nbss and red to normal Nbss in AC alloy. (c) Element X versus Cr in Nbss, data for X = B (brown) or Ti (purple) in the Nbss of the HT alloys TT2, TT4 and TT8. (d) Ti + B + X (X = Al, Cr) versus VEC of Nbss in the HT alloys TT2, TT3, TT4 and TT8, purple X = Al, alloys TT3, TT4, TT8, pink X = Cr, alloys TT2, TT4, TT8, (e) Ti + Cr versus VEC and (f) Ti versus VEC of Nbss, HT alloys TT2, TT4, TT8.
Materials 14 06101 g004aMaterials 14 06101 g004bMaterials 14 06101 g004c
Figure 5. Maps of the 5-3 silicide in the AC and HT boron-containing alloys TT2, TT3, TT4 and TT8, i.e., of the T2 silicide, and the reference B-free alloys KZ4, KZ5, KZ7 and JG3, i.e., of Nb5Si3. (a) and (b) Δχ versus VEC, (c) VEC versus <Nb> and (d) Δχ versus <Nb>. Diamonds for B-containing alloys, i.e., data for T2, and pink filed circles for the B free alloys, i.e., data for Nb5Si3. (a) and (d) data for T2, Ti-rich T2, Nb5Si3 and Ti-rich Nb5Si3. (b) and (c) data for T2 and Nb5Si3 in the aforementioned alloys. In (b) and (c) green for TT2 and KZ4, red for TT3 and KZ7, purple for TT4 and KZ5, and blue for TT8 and JG3. <Nb> means Nb and other elements that substitute Nb in silicide. For all data in (a) R2 = 0.5173 for linear fit. The dashed lines in (a) delineate the “territory” occupied by the T2 silicide in the B containing alloys TT2, TT3, TT4 and TT8 (defined by Δχ and VEC approximately less than 0.303 and 4.36).
Figure 5. Maps of the 5-3 silicide in the AC and HT boron-containing alloys TT2, TT3, TT4 and TT8, i.e., of the T2 silicide, and the reference B-free alloys KZ4, KZ5, KZ7 and JG3, i.e., of Nb5Si3. (a) and (b) Δχ versus VEC, (c) VEC versus <Nb> and (d) Δχ versus <Nb>. Diamonds for B-containing alloys, i.e., data for T2, and pink filed circles for the B free alloys, i.e., data for Nb5Si3. (a) and (d) data for T2, Ti-rich T2, Nb5Si3 and Ti-rich Nb5Si3. (b) and (c) data for T2 and Nb5Si3 in the aforementioned alloys. In (b) and (c) green for TT2 and KZ4, red for TT3 and KZ7, purple for TT4 and KZ5, and blue for TT8 and JG3. <Nb> means Nb and other elements that substitute Nb in silicide. For all data in (a) R2 = 0.5173 for linear fit. The dashed lines in (a) delineate the “territory” occupied by the T2 silicide in the B containing alloys TT2, TT3, TT4 and TT8 (defined by Δχ and VEC approximately less than 0.303 and 4.36).
Materials 14 06101 g005aMaterials 14 06101 g005b
Figure 6. Vickers hardness (HV) of Nbss in HT alloys versus the parameter VEC of the solid solution. (a) alloys TT2, TT4, TT8 (red), KZ4, KZ5 and JG3 (blue), all data R2 = 0.7871 (b) alloys TT3, TT4, TT8 (red), KZ7, KZ5 and JG3 (blue), all data R2 = 0.8277. (c) Vickers hardness of Nbss in AC (green) and HT (purple) alloys TT2, TT4, TT8, all data R2 = 0.8962.
Figure 6. Vickers hardness (HV) of Nbss in HT alloys versus the parameter VEC of the solid solution. (a) alloys TT2, TT4, TT8 (red), KZ4, KZ5 and JG3 (blue), all data R2 = 0.7871 (b) alloys TT3, TT4, TT8 (red), KZ7, KZ5 and JG3 (blue), all data R2 = 0.8277. (c) Vickers hardness of Nbss in AC (green) and HT (purple) alloys TT2, TT4, TT8, all data R2 = 0.8962.
Materials 14 06101 g006
Figure 7. Vickers hardness (HV) of Nbss in the HT alloys TT2, TT3, TT4, TT8 versus (a) Ti + B + X, (b) Ti + X, (X = Al (blue), Cr (red)), (c) Ti/Cr for the alloys TT2, TT4, TT8, and (d) HV of Nbss in the HT alloys TT3, TT4, TT8 (green) and KZ7, KZ5 and JG3 (brown).
Figure 7. Vickers hardness (HV) of Nbss in the HT alloys TT2, TT3, TT4, TT8 versus (a) Ti + B + X, (b) Ti + X, (X = Al (blue), Cr (red)), (c) Ti/Cr for the alloys TT2, TT4, TT8, and (d) HV of Nbss in the HT alloys TT3, TT4, TT8 (green) and KZ7, KZ5 and JG3 (brown).
Materials 14 06101 g007aMaterials 14 06101 g007b
Figure 8. (a) to (c) Vickers hardness (HV) and (d) room temperature specific strength calculated from hardness (σHV/ρ) versus the parameters (a), (d) VEC, (b) δ and (c) Δχ of the TT2, TT3, TT4, TT8, KZ4, KZ5, KZ7 and JG3 alloys. In (a) to (c) the data is for the AC and HT conditions and in (d) the data is for the AC condition. Filled circles green TT2 and KZ4, red TT3 and KZ7, purple TT4 and KZ5, and blue TT8 and JG3. In (b) and (c) ellipses enclose the B containing alloys. In (a) and (d) the R2 values are for the parabolic fit of data. In (a) data for the alloys TT2, TT3, TT4 and TT8 with R2 = 0.998 and R2 = 0.9046 for the AC and HT conditions, respectively and with R2 = 0.9922 and R2 = 0.9908 respectively for the AC and HT alloys KZ4, KZ5, KZ7 and JG3. In (d) R2 = 0.9993 and R2 = 0.9888 respective for the AC alloys TT2, TT3, TT4, TT8 and KZ4, KZ5, KZ7, JG3. In (a) and (d) green arrows indicate the effect of B addition.
Figure 8. (a) to (c) Vickers hardness (HV) and (d) room temperature specific strength calculated from hardness (σHV/ρ) versus the parameters (a), (d) VEC, (b) δ and (c) Δχ of the TT2, TT3, TT4, TT8, KZ4, KZ5, KZ7 and JG3 alloys. In (a) to (c) the data is for the AC and HT conditions and in (d) the data is for the AC condition. Filled circles green TT2 and KZ4, red TT3 and KZ7, purple TT4 and KZ5, and blue TT8 and JG3. In (b) and (c) ellipses enclose the B containing alloys. In (a) and (d) the R2 values are for the parabolic fit of data. In (a) data for the alloys TT2, TT3, TT4 and TT8 with R2 = 0.998 and R2 = 0.9046 for the AC and HT conditions, respectively and with R2 = 0.9922 and R2 = 0.9908 respectively for the AC and HT alloys KZ4, KZ5, KZ7 and JG3. In (d) R2 = 0.9993 and R2 = 0.9888 respective for the AC alloys TT2, TT3, TT4, TT8 and KZ4, KZ5, KZ7, JG3. In (a) and (d) green arrows indicate the effect of B addition.
Materials 14 06101 g008aMaterials 14 06101 g008b
Figure 9. Maps of the parameters VECalloy, δalloy and Δχalloy with sums or ratios of Ti, Cr or B in AC and HT alloys TT2, TT4, TT8 and “equivalent” B free alloys KZ4, KZ5 and JG3. R2 values for linear or parabolic fit of data. (a) VECalloy versus (Ti + Cr)alloy, (b) δalloy versus (Ti + Cr)alloy, (c) Δχalloy versus (Ti + Cr)alloy, (d) VEC versus Ti/Cr, (e) δ versus Ti/Cr, (f) Δχ versus Ti/Cr, (g) VEC versus Ti + Cr + B, (h) δ versus Ti + Cr + B and ((i) Δχ versus Ti + Cr + B. (a) to (f) data for the alloys TT2, KZ4, TT4, KZ5, TT8 and JG3, (g) to (i) data for the alloys TT2, TT4, TT8. (a,b,d,e) colours as follows: green for TT2 and KZ4, purple for TT4 and KZ5, and blue for TT8 and JG3. (g) to (i) triangles for TT8, squares for TT4, and circles for TT2. (c) and (f) green colour for all alloys. In (a) to (f) diamonds for B containing alloys.
Figure 9. Maps of the parameters VECalloy, δalloy and Δχalloy with sums or ratios of Ti, Cr or B in AC and HT alloys TT2, TT4, TT8 and “equivalent” B free alloys KZ4, KZ5 and JG3. R2 values for linear or parabolic fit of data. (a) VECalloy versus (Ti + Cr)alloy, (b) δalloy versus (Ti + Cr)alloy, (c) Δχalloy versus (Ti + Cr)alloy, (d) VEC versus Ti/Cr, (e) δ versus Ti/Cr, (f) Δχ versus Ti/Cr, (g) VEC versus Ti + Cr + B, (h) δ versus Ti + Cr + B and ((i) Δχ versus Ti + Cr + B. (a) to (f) data for the alloys TT2, KZ4, TT4, KZ5, TT8 and JG3, (g) to (i) data for the alloys TT2, TT4, TT8. (a,b,d,e) colours as follows: green for TT2 and KZ4, purple for TT4 and KZ5, and blue for TT8 and JG3. (g) to (i) triangles for TT8, squares for TT4, and circles for TT2. (c) and (f) green colour for all alloys. In (a) to (f) diamonds for B containing alloys.
Materials 14 06101 g009aMaterials 14 06101 g009bMaterials 14 06101 g009cMaterials 14 06101 g009d
Figure 10. Densities of as cast alloys KZ4, KZ7, KZ5 (dark blue, 1, 4, 7), ZF4, ZF5, ZF6 (red, 2, 5, 8) and TT2, TT3, TT4 (green, 3, 6, 9). See Appendix A for nominal compositions of alloys.
Figure 10. Densities of as cast alloys KZ4, KZ7, KZ5 (dark blue, 1, 4, 7), ZF4, ZF5, ZF6 (red, 2, 5, 8) and TT2, TT3, TT4 (green, 3, 6, 9). See Appendix A for nominal compositions of alloys.
Materials 14 06101 g010
Figure 11. Room temperature Vickers hardness of AC and HT alloys. Odd numbers AC alloys, even numbers HT alloys. TT2 (1, 2), ZF4 (3, 4), TT3 (5, 6), ZF5 (7, 8), TT4 (9, 10), ZF6 (11, 12). See Appendix A for nominal compositions of alloys.
Figure 11. Room temperature Vickers hardness of AC and HT alloys. Odd numbers AC alloys, even numbers HT alloys. TT2 (1, 2), ZF4 (3, 4), TT3 (5, 6), ZF5 (7, 8), TT4 (9, 10), ZF6 (11, 12). See Appendix A for nominal compositions of alloys.
Materials 14 06101 g011
Figure 12. Comparison of mass changes of B-containing alloys TT2, TT3, TT4 and TT8 with reference alloys KZ4, KZ5, KZ7 and JG3. For isothermal oxidation at 800 and 1200 °C. Arrows indicate direction of mass change at 800 °C (ad) and 1200 °C (eh).
Figure 12. Comparison of mass changes of B-containing alloys TT2, TT3, TT4 and TT8 with reference alloys KZ4, KZ5, KZ7 and JG3. For isothermal oxidation at 800 and 1200 °C. Arrows indicate direction of mass change at 800 °C (ad) and 1200 °C (eh).
Materials 14 06101 g012aMaterials 14 06101 g012b
Figure 13. Mass change (ΔW/A) of the alloys TT2, TT3, TT4, TT8 and their basis/reference alloys KZ4, KZ5, KZ7 and JG3 versus the parameters (a,c) VEC and (b,d) δ for isothermal oxidation (a,b) at 800 °C and (c,d) at 1200 °C. Colours as follows: green for TT2 and KZ4, red for TT3 and KZ7, purple for TT4 and KZ5, and blue for TT8 and JG3. Diamonds for B containing alloys.
Figure 13. Mass change (ΔW/A) of the alloys TT2, TT3, TT4, TT8 and their basis/reference alloys KZ4, KZ5, KZ7 and JG3 versus the parameters (a,c) VEC and (b,d) δ for isothermal oxidation (a,b) at 800 °C and (c,d) at 1200 °C. Colours as follows: green for TT2 and KZ4, red for TT3 and KZ7, purple for TT4 and KZ5, and blue for TT8 and JG3. Diamonds for B containing alloys.
Materials 14 06101 g013aMaterials 14 06101 g013b
Table 1. Nominal and actual composition (at.%) of as cast (AC) and heat-treated (HT) alloys.
Table 1. Nominal and actual composition (at.%) of as cast (AC) and heat-treated (HT) alloys.
AlloyConditionElement
NbTiSiAlCrBMo
TT2nominal482416-57-
-AC47.824.216.3-5.26.5-
-HT47.32416.5-5.36.9-
TT3nominal4824165-7-
-AC49.323.615.44.4-7.3-
-HT49.523.215.64.4-7.3-
TT4nominal402418558-
-AC42.424.615.755.46.9-
-HT40.72417.34.84.98.3-
TT8nominal42.524173.5562
-AC43.42317.23.54.962
-HT42.923.717.23.34.95.92.1
Table 2. Density of alloys, vol.% Nbss, hardness * of alloys, microhardness * of Nbss and T2 silicide.
Table 2. Density of alloys, vol.% Nbss, hardness * of alloys, microhardness * of Nbss and T2 silicide.
AlloyHardness HValloyρ (g/cm3)Vol.% NbssMicrohardness HVphase
NbssT2
ACHTACHTACHTACHTACHT
TT2688 ± 42
622–734
680 ± 28
624–708
6.716.723738472 ± 18
443–496
419 ± 39
377–495
1346 ± 70
1202–1445
1167 ± 84
1015–1265
TT3630 ± 86
494–757
571 ± 54
501–659
6.526.563842521 ± 34
472–577
379 ± 19
352–411
1232 ± 72
1116–1334
1163 ± 80
1061–1332
TT4720 ± 70
642–879
607 ± 21
590–659
6.416.413039563 ± 37
503–631
467 ± 15
450–496
1247 ± 55
1172–1334
1239 ± 40
1200–1332
TT8744 ± 60
673–842
693 ± 28
622–717
6.466.443938531 ± 26
487–576
461 ± 25
417–495
1316 ± 37
1265–1369
1209 ± 48
1143–1299
* given as the average value, standard deviation, and maximum and minimum measured values.
Table 3. Macrosegregation (at.%) of solutes MACX (X = Al, B, Cr, Si, Ti) in the cast alloys, where MACX = CmaxX − CminX [19].
Table 3. Macrosegregation (at.%) of solutes MACX (X = Al, B, Cr, Si, Ti) in the cast alloys, where MACX = CmaxX − CminX [19].
AlloyMACX (at.%)
AlBCrSiTi
TT2-4.22.83.13.2
TT32.74.2-4.53.4
TT41.12.91.44.73.3
TT81.14.91.31.32.8
TT1 [12]-4.4-4.15.5
Table 4. Phases in the as cast (AC) and heat-treated (HT) alloys according to the XRD and EPMA data.
Table 4. Phases in the as cast (AC) and heat-treated (HT) alloys according to the XRD and EPMA data.
Alloy and ConditionPhase
NbssT2Cr & Ti Rich PhaseTi Rich PhaseC14-LavesNb3SiD88Nbss + T2 EutecticTiN
TT2-ACX *X *XXXX-X-
TT2-HT XX *------X °
TT3-ACX *X *-----X-
TT3-HT +XX *-------
TT4-ACX *X *----XX-
TT4-HT +XX----X--
TT8-ACX *X *---XXX-
TT8-HT +XX *----X-X °
* indicates the presence also of Ti-rich phase (see Table 5), + 1500 °C/100 h, 1200 °C/100 h, o indicates that alloy was contaminated by nitrogen.
Table 5. EPMA data for the chemical composition (at.%) of phases in AC and HT alloys.
Table 5. EPMA data for the chemical composition (at.%) of phases in AC and HT alloys.
Alloy and ConditionPhaseElement
NbTiSiAlBCrMo
TT2-ACNbss57.2–63.2
60.3 ± 2.4
23.7–29
26.6 ± 1.7
1.4–1.9
1.6 ± 0.2
-3.6–6.3
5 ± 0.2
5.3–7.9
6.5 ± 1
-
-Ti rich Nbss38.8–46.6
42.5 ± 3.8
36.9–43.9
40.7 ± 1.7
1.6–3.5
2.4 ± 0.2
-0.6–3.3
1.8 ± 0.2
10.1–14.1
12.6 ± 2.3
-
-Phase rich
in Cr & Ti
14.8–21.9
18.9 ± 2.6
40.2–53.9
48.3 ± 1.4
3.4–12.9
7.1 ± 2.7
--23.4–28.5
25.7 ± 4.5
-
-T246–48.1
47.1 ± 0.6
13.4–15.4
14.3 ± 0.9
23.4–26.4
25.3 ± 1
-10.9–14.9
12.9 ± 1.1
0.2–0.7
0.4 ± 0.1
-
-Ti rich T239.1–43.7
41.6 ± 1.2
18.6–23.8
20.8 ± 1.6
28.1–30.3
29.3 ± 0.7
-5.9–9.4
7.8 ± 1
0.2–0.8
0.5 ± 0.1
-
TT3-ACNbss52.9–59.4
55.8 ± 0.6
28.6–32.6
30.6 ± 1.2
1.6–2
1.8 ± 0.1
3.9–8.4
6.8 ± 2.2
4–6
5 ± 0.6
--
-Ti rich Nbss43.4–49.9
47.7 ± 0.6
38.7–47.8
42.7 ± 1.6
1.7–2
1.9 ± 0.1
3.3–5.4
4.5 ± 2.4
1.9–4.4
3.2 ± 0.7
--
-T246–48.3
46.9 ± 0.4
13.3–15.6
14.4 ± 0.2
22.5–26.7
25 ± 1.2
0.4–1.2
0.8 ± 0.1
10.8–16.2
12.9 ± 1.5
--
-Ti rich T241.3–45.1
42 ± 1.4
18.2–19.9
19 ± 0.3
29.1–30.4
29.8 ± 0.4
0.6–2.7
1.7 ± 0.6
6.6–8.6
7.5 ± 0.5
--
TT4Nbss46.4–50.1
48.3 ± 2.1
29.4–31.6
30.6 ± 1.7
1.2–1.7
1.4 ± 0.1
7.1–7.7
7.4 ± 0.3
2.5–3.9
3.3 ± 0.3
7.9–10.1
9 ± 0.4
-
-Ti rich Nbss32.7–39.4
35.6 ± 1.1
37–42.5
39.7 ± 0.5
1.1–1.5
1.3 ± 0.1
6.7–7.3
7 ± 0.4
0.3–1.2
0.7 ± 0.4
14.1–16.9
15.7 ± 1.4
-
-T240.5–42.6
41.4 ± 0.3
19–20.3
19.7 ± 0.4
27.5–29.9
29.1 ± 0.8
1.7–2.7
2.3 ± 0.3
5.2–8.3
6.8 ± 0.4
0.4–1.1
0.7 ± 0.1
-
-Ti rich T228.5–35.8
32.5 ± 1
26.2–33.5
29.3 ± 0.9
27.4–29.3
28.3 ± 0.8
3.7–4.3
4 ± 0.3
3.2–5.5
4.4 ± 0.4
0.8–2.2
1.5 ± 0.4
-
-D8844.5–46.9
45.9 ± 0.6
11.7–13.3
12.5 ± 0.6
14.4–16
15 ± 0.8
-23.5–27
25.6 ± 0.4
0.6–1.4
1 ± 0.3
-
TT8-ACNbss42.4–49.9
45.9 ± 2.5
26.9–30.9
28.8 ± 1.1
1.1–1.5
1.3 ± 0.3
6.8–8.5
7.6 ± 0.4
0–5.4
1.8 ± 1.4
9.1–11.5
10.6 ± 1.4
3.5–4.5
4 ± 0.6
-Ti rich Nbss30.8–38
34.5 ± 0.7
36.4–41.5
38.4 ± 2.1
1–1.4
1.2 ± 0.3
6–7.3
6.8 ± 0.7
0–3.5
1.1 ± 0.8
14.2–16.6
15.6 ± 2.2
2–2.8
2.4 ± 0.1
-T236.7–43.5
40.5 ± 1.2
18.2–20.8
19.1 ± 0.4
24–28
25.6 ± 4.9
2.6–3.5
2.9 ± 0.2
6.7–15.5
10.4 ± 6.3
0.6–1.1
0.8 ± 0.2
0.6–0.7
0.7 ± 0.1
-Ti rich T229.2–32.1
30.7 ± 1.3
29.4–31.5
30.2 ± 0.9
24.7–27.8
26.4 ± 3.5
3–4.2
3.3±0.5
6.5–9.5
8 ± 1.1
0.3–1
0.9 ± 0.3
0.3–0.7
0.5 ± 0.2
-D8841.9–45.2
44.7 ± 2
9.2–12.3
10.2 ± 0.6
11–13.5
12.4 ± 0.9
-26.4–33.7
30 ± 2.6
0.8–1.3
1 ± 0.2
1.6–1.8
1.7 ± 0.2
TT2-HTNbss52.1–55.2
53.2 ± 1.2
30.1–33.6
31.9 ± 1.6
0.3–0.5
0.4 ± 0.1
-2–4.3
3.2 ± 0.5
10.2–12
11.3 ± 0.2
-
-T2 *46.9–48.6
47.8 ± 1.2
13.7–15.2
14.4 ± 1
23.3–26
24.5 ± 1.2
-10.7–14.8
12.7 ± 1.5
0.3–0.8
0.6 ± 0.1
-
TT3-HTNbss54.8–57.9
56.4 ± 1
29.2–32
30.7 ± 1
0.3–0.5
0.4 ± 0.1
7.5–8.3
7.8 ± 0.6
3.8–5.6
4.7 ± 0.6
--
-T241.8–46.2
44.1 ± 2.4
16.1–19.7
17.4 ± 2.2
25.4–28
26.9 ± 2
0.8–1.8
1.4 ± 0.9
9–11.7
10.2 ± 2.6
--
-Ti rich T234–36.6
34.8 ± 1.3
25–29
27.4 ± 1
28–29.5
28.9 ± 0.7
3.7–4.5
4.2 ± 0.5
3.8–5.9
4.7 ± 0.4
--
TT4-HTNbss48.5–50.5
49.8 ± 0.8
28.1–29.5
28.6 ± 0.6
0.4–0.7
0.5 ± 0.1
7.3–7.8
7.6 ± 0.2
1.5–4.3
2.8 ± 1
10.4–11
10.7 ± 0.2
-
-T235.8–40
37.7 ± 1.9
19.7–24.6
22.3 ± 1.9
29.4–31.2
30.2 ± 0.8
2.3–3.8
3.3 ± 0.5
4.2–6.3
5.5± 0.8
0.7–1.4
1 ± 0.2
-
-D8842.7–44.5
43.6 ± 0.8
11.6–12.4
11.9 ± 0.3
12.9–14.2
13.4 ± 0.5
-28–30.7
29.2 ± 1
1.6–2.2
1.9 ± 0.3
-
TT8-HTNbss46.2–48.7
45.6 ± 1
23.9–31.5
29.8 ± 2.2
0.4–0.6
0.5 ± 0.1
7.2–8.2
7.6 ± 0.5
0–4.8
1 ± 0.8
10.5–11.8
11.2 ± 0.7
4.1–4.4
4.3 ± 0.1
-T235.8–44.5
41 ± 4.6
18.7–21.5
20.1 ± 1.4
27.1–33.2
29.3 ± 3.4
2.7–4.3
3.3 ± 0.8
0–8.7
4.7 ± 4.4
0.4–1.9
1.1 ± 0.8
0.3–0.7
0.5 ± 0.2
-Ti rich T230.9–33.7
31.6 ± 1.2
25.9–31.2
28.1 ± 2
26.4–29.6
28 ± 1.3
3.3–3.6
3.5 ± 0.2
3.3–11
6.8 ± 4.6
1.1–1.8
1.5 ± 0.3
0.4–0.5
0.5 ± 0.02
-D8841.2–48.9
44.2 ± 4.3
11.4–12.6
12.1 ± 0.7
12.4–4.9
13.5 ± 1.5
-19.2–31
26.5 ± 6.4
1.5–2.3
2 ± 0.5
1.6–1.9
1.7 ± 0.1
* see text.
Table 6. Oxidation rate constants and mass changes of the alloys after isothermal oxidation for 100 h at 800 and 1200 °C.
Table 6. Oxidation rate constants and mass changes of the alloys after isothermal oxidation for 100 h at 800 and 1200 °C.
AlloyOxidation Rate ConstantMass Change
ΔW/A (mg/cm2)
Pest OxidationScale Spallation
800 °C
kl (g/cm2s)
1200 °C
kp (g2/cm4s)
800 °C1200 °C800 °C800 °C1200 °C
MASC1.53 × 10−71.58 × 10−836 (≤65 h)80MC *-Yes
TT11.86 × 10−71.53 × 10−86380.3NoYesYes
TT21.89 × 10−73.32 × 10−861.4105.6NoYesYes
TT31.22 × 10−71.21 × 10−838.666.1NoYesYes
TT48.9 × 10−83.4 × 10−927.934NoYesYes
TT83 × 10−93.3 × 10−91.430NoNoNo
* MC = Maltese cross.
Table 7. Comparison of the macrosegregation (MACX) of X = B, Si or Ti in the B containing alloys of this work and their basis/reference alloys KZ3, KZ4, KZ5, KZ7 [16] and JG3 [17] (see Appendix A). Large button ingots (0.6 kg) of all alloys were prepared using arc melting. Note that the table includes data for the alloy TT1 (Nb-24Ti-18Si-8B [12]) and its basis alloy KZ3 (Nb-24Ti-18Si [16]).
Table 7. Comparison of the macrosegregation (MACX) of X = B, Si or Ti in the B containing alloys of this work and their basis/reference alloys KZ3, KZ4, KZ5, KZ7 [16] and JG3 [17] (see Appendix A). Large button ingots (0.6 kg) of all alloys were prepared using arc melting. Note that the table includes data for the alloy TT1 (Nb-24Ti-18Si-8B [12]) and its basis alloy KZ3 (Nb-24Ti-18Si [16]).
AlloyMACSi (at.%)AlloyMACB
(at.%)
AlloyMACTi
(at.%)
TT4 Materials 14 06101 i0014.7TT8 Materials 14 06101 i0024.9TT1 Materials 14 06101 i0035.5
TT34.5TT14.4TT33.4
TT14.1TT24.2TT43.3
TT23.1TT34.2TT23.2
JG32.6TT42.9KZ33.1
KZ72.3--TT82.8
KZ41.9--KZ72.3
KZ31.6--JG31.5
TT81.3--KZ41.4
KZ51.3--KZ51.4
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Thandorn, T.; Tsakiropoulos, P. The Effect of Boron on the Microstructure and Properties of Refractory Metal Intermetallic Composites (RM(Nb)ICs) Based on Nb-24Ti-xSi (x = 16, 17 or 18 at.%) with Additions of Al, Cr or Mo. Materials 2021, 14, 6101. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14206101

AMA Style

Thandorn T, Tsakiropoulos P. The Effect of Boron on the Microstructure and Properties of Refractory Metal Intermetallic Composites (RM(Nb)ICs) Based on Nb-24Ti-xSi (x = 16, 17 or 18 at.%) with Additions of Al, Cr or Mo. Materials. 2021; 14(20):6101. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14206101

Chicago/Turabian Style

Thandorn, Tophan, and Panos Tsakiropoulos. 2021. "The Effect of Boron on the Microstructure and Properties of Refractory Metal Intermetallic Composites (RM(Nb)ICs) Based on Nb-24Ti-xSi (x = 16, 17 or 18 at.%) with Additions of Al, Cr or Mo" Materials 14, no. 20: 6101. https://0-doi-org.brum.beds.ac.uk/10.3390/ma14206101

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.